A monodisperse hollow polystyrene-divinylbenzene composite microsphere, preparation method thereof and application in enzyme-linked immunosorbent assay
Monodispersed hollow polystyrene-divinylbenzene composite microspheres were prepared by dispersion polymerization, which solved the problem of complex template removal steps and uneven particle size, and achieved efficient and low-cost hollow microsphere preparation with high specific surface area and thermal stability.
Patent Information
- Application Number
- CN202211096145.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-08
AI Technical Summary
In the prior art, when preparing monodispersed hollow polymer microspheres, the template removal steps are complex and costly, and it is difficult to achieve the preparation of hollow nanometer microspheres with uniform particle size and adjustable size.
By using the dispersion polymerization method, the molecular weight and pore-generating agent ratio of polystyrene seed microspheres are regulated, and the emulsion polymerization reaction is used to polymerize under an inert gas atmosphere to form monodispersed hollow polystyrene-divinylbenzene composite microspheres, template Automatic removal during the reaction process simplifies the preparation process.
The preparation of monodispersed hollow microspheres with high specific surface area and good thermal stability is achieved, which simplifies the process flow, reduces costs, and can regulate the particle size and cavity size of the microspheres.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0003838726370000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biological nanomaterials, and in particular relates to a monodisperse hollow polystyrene-divinylbenzene composite microsphere, a preparation method thereof and an application thereof in enzyme-linked immunosorbent assay. Background Art
[0002] In recent years, with the continuous development and improvement of polymer microsphere preparation technology, polymer microspheres of different structures, different particle sizes and different types have been widely used in architectural coating production, building material additives, paper surface processing and other fields due to their stable physical and chemical properties and easy preparation. Among them, monodisperse hollow polymer microspheres have high specific surface area, large loading cavity, low density and good suspension due to their special hollow structure. Therefore, this kind of monodisperse hollow polymer microspheres with special properties can be applied to enzyme-linked immunosorbent assay, microreactors, drug delivery, separation and purification of bioactive substances and other high-tech fields. At present, how to simply and quickly prepare monodisperse hollow polymer microspheres has become a hot topic for scholars.
[0003] At present, a variety of methods for preparing hollow spheres have been developed, including hard template method, soft template method and template-free method. Among them, the hard template method has the advantages of simple operation, uniform particle size, and easy regulation, but its template removal is relatively complicated. Some need to be calcined to remove, such as using polymers as templates, and some need to be etched to remove, such as using iron oxide microspheres as templates. At the same time, the hard template method requires the preparation of the template first, then wrapping it on the surface, and finally removing the template. The operation steps are cumbersome and the cost is high; the template may agglomerate during the wrapping process, and it is easy to destroy the structure of the nanomaterial and introduce impurities when removing the template. Soft templates are often aggregated by surfactant molecules, mainly including various ordered polymers formed by amphiphilic molecules, such as liquid crystals, vesicles, micelles, microemulsions, self-assembled membranes, and self-assembled structures of biomolecules and polymers. Weak interactions between or within molecules are the forces that maintain the template, thereby forming aggregates with different spatial structural characteristics. The soft template has a variety of morphologies when preparing nanomaterials, and is easy to construct and does not require complex equipment. However, compared with hard templates, the stability of the soft template structure is poor, so the template efficiency is not high enough. In summary, in order to prepare hollow nanospheres with uniform particle size and adjustable size, the template removal step is indispensable in the process of preparing hollow microspheres using the traditional template method. Therefore, how to use the template to prepare hollow spheres and remove the template simply and quickly has become the focus and difficulty of the research. Summary of the invention
[0004] The purpose of the present invention is to provide a monodisperse hollow polystyrene-divinylbenzene composite microsphere, a preparation method thereof and application in enzyme-linked immunosorbent assay. The prepared polystyrene-divinylbenzene composite microspheres of the present invention have large specific surface area, high thermal stability, high loading capacity and good suspension.
[0005] The present invention provides a method for preparing monodisperse hollow polystyrene-divinylbenzene composite microspheres, comprising the following steps:
[0006] A) mixing polystyrene seed microspheres with a molecular weight of 30,000 to 40,000, a dispersant and an emulsifier, and emulsifying to obtain an emulsified solution of polystyrene seed microspheres;
[0007] B) uniformly mixing an initiator, a styrene monomer, a divinylbenzene monomer and a porogen, adding the mixture to the emulsified solution of the polystyrene seed microspheres, and performing a polymerization reaction after swelling for 2 to 10 hours under an inert gas atmosphere, washing and drying the obtained product to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres.
[0008] Preferably, the polystyrene seed microspheres are prepared according to the following steps:
[0009] Adding polyvinyl pyrrolidone, styrene monomer and initiator into an alcohol-water mixed solution, reacting at 65-85° C. for 2-10 hours in an inert gas atmosphere to obtain polystyrene seed microspheres;
[0010] The initiator is one or more of an azo initiator, an organic peroxide initiator, and an inorganic peroxide initiator.
[0011] Preferably, the mass ratio of alcohol to water in the alcohol-water mixed solution is (2-4):1; the molar ratio of the styrene monomer to the initiator is (10-20):1; and the mass ratio of the polyvinyl pyrrolidone to the styrene monomer is 1:(3-8).
[0012] Preferably, the dispersant in step A) is one or more of polyvinyl pyrrolidone, polyvinyl alcohol, and hydroxyethyl cellulose; and the emulsifier is one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
[0013] Preferably, in the emulsified solution of polystyrene seed microspheres, the mass concentration of polystyrene seed microspheres is 2-10 mg / mL; the mass concentration of the dispersant is 1-8 mg / mL; and the mass concentration of the emulsifier is 0.2-5 mg / mL.
[0014] Preferably, the initiator in step B) is one or more of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator and a redox system initiator;
[0015] The porogen in step B) is one or more of toluene, acetone and cyclohexane.
[0016] Preferably, the ratio of the sum of the mass of the styrene monomer and the divinylbenzene monomer in step B) to the mass of the initiator in step B) is (20-40):1; the ratio of the sum of the mass of the styrene monomer and the divinylbenzene monomer in step B) to the mass of the porogen is (1-5):(1-4).
[0017] Preferably, the polymerization reaction temperature in step B) is 65 to 85° C. and the polymerization reaction time is 5 to 10 hours.
[0018] The present invention provides monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared by the preparation method described above.
[0019] The present invention provides the use of the monodisperse hollow polystyrene-divinylbenzene composite microspheres as described above in enzyme-linked immunosorbent assay.
[0020] Preferably, the monodisperse hollow polystyrene-divinylbenzene composite microspheres are sequentially nitrated, reduced, magnetically deposited with superparamagnetic ferroferric oxide nanoparticles, coated with a polymer layer, and surface carboxylated to obtain hollow spherical chemiluminescent magnetic beads for use in enzyme-linked immunosorbent assay.
[0021] The present invention provides a method for preparing monodisperse hollow polystyrene-divinylbenzene composite microspheres, comprising the following steps: A) mixing polystyrene seed microspheres with a molecular weight of 30,000 to 40,000, a dispersant and an emulsifier, and obtaining an emulsified solution of polystyrene seed microspheres after emulsification; B) uniformly mixing an initiator, a styrene monomer, a divinylbenzene monomer and a porogen, adding the mixture to the emulsified solution of the polystyrene seed microspheres, and performing a polymerization reaction after swelling for 2 to 10 hours under an inert gas atmosphere to obtain a product, which is then washed and dried to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres. The concept and technical core of the present invention are: (1) using a dispersion polymerization method to adjust relevant parameters to prepare a microsphere with a molecular weight of 10 4(2) After adding the corresponding proportion of swelling agent, porogen and other solvents by emulsion polymerization, the seed microspheres with larger molecular weight are relatively difficult to swell at room temperature and only swell on the surface of the seed microspheres; when the temperature is raised, the reaction is preferentially carried out at the periphery to form a dense shell layer, while the hydrophobic porogen that does not participate in the reaction cannot dissolve the shell layer of the cross-linked composite microspheres and can only be squeezed into the interior of the microspheres. The porogen can dissolve the linear polystyrene seed microspheres inside to form a hollow structure. (3) Changing the molecular weight of the seed microspheres can control the size of the composite microsphere cavity; (4) Changing the proportion of the porogen can also control the size of the composite microsphere cavity; (5) The template can be removed during the reaction without the need for additional steps; (6) The swollen part of the seed undergoes a cross-linking reaction to form a shell layer, and the unswollen part is subsequently dissolved to form an inner cavity of the corresponding volume. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1 The solution appearance of the polystyrene seed microspheres (I) and the polystyrene-divinylbenzene composite microspheres (II) prepared in Example 1;
[0024] Figure 2 This is a microscope photo of the polystyrene seed microspheres prepared in Example 1;
[0025] Figure 3 This is the particle size distribution diagram of the polystyrene seed microspheres prepared in Example 1;
[0026] Figure 4 This is a microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1;
[0027] Figure 5 This is a scanning electron microscope photograph of the polystyrene seed microspheres prepared in Example 1;
[0028] Figure 6 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1;
[0029] Figure 7 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1 after grinding;
[0030] Figure 8 This is a scanning electron microscope photograph of the polystyrene seed microspheres prepared in Example 2;
[0031] Fig. 9 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 2;
[0032] Fig.10 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 2 after grinding;
[0033] Fig.11 This is a scanning electron microscope photograph of the polystyrene seed microspheres prepared in Example 3;
[0034] Fig.12 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 3;
[0035] Fig.13 This is a scanning electron microscope photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 3 after grinding;
[0036] Fig.14 is a scanning electron microscope photograph of the carboxylated hollow magnetic beads prepared in the application example of the present invention;
[0037] Fig.15 The magnetic response performance of the carboxylated hollow magnetic beads prepared in the application example of the present invention. DETAILED DESCRIPTION
[0038] The present invention provides a method for preparing monodisperse hollow polystyrene-divinylbenzene composite microspheres, comprising the following steps:
[0039] A) mixing polystyrene seed microspheres with a molecular weight of 30,000 to 40,000, a dispersant and an emulsifier, and emulsifying to obtain an emulsified solution of polystyrene seed microspheres;
[0040] B) uniformly mixing an initiator, a styrene monomer, a divinylbenzene monomer and a porogen, adding the mixture to the emulsified solution of the polystyrene seed microspheres, and performing a polymerization reaction after swelling for 2 to 10 hours under an inert gas atmosphere, washing and drying the obtained product to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres.
[0041] The present invention first prepares the polystyrene seed microspheres according to the following steps:
[0042] Polyvinyl pyrrolidone, styrene monomer and initiator are added into an alcohol-water mixed solution, and reacted at 65-85° C. for 2-10 hours in an inert gas atmosphere to obtain polystyrene seed microspheres.
[0043] In the present invention, the initiator is preferably one or more of an azo initiator, an organic peroxide initiator, and an inorganic peroxide initiator; more preferably one or more of azobisisobutyronitrile (AIBN), dibenzoyl peroxide (BPO) and potassium persulfate; the alcohol in the alcohol aqueous solution is preferably anhydrous methanol and / or anhydrous ethanol; the mass ratio of alcohol to water in the alcohol aqueous solution is preferably (2-4): 1, such as 2:1, 3:1 or 4:1, preferably a range value with any of the above values as the upper or lower limit; the inert gas is preferably one or more of nitrogen, helium and argon.
[0044] In the present invention, the molar ratio of the styrene monomer to the initiator is preferably (10-20):1, more preferably (13-18):1, such as 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 9:1, 20:1, preferably a range value with the above arbitrary numerical values as the upper or lower limit; the mass ratio of the polyvinyl pyrrolidone to the styrene monomer is preferably 1:(3-8), more preferably 1:(5-6), such as 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, preferably a range value with the above arbitrary numerical values as the upper or lower limit.
[0045] In the present invention, the reaction temperature is preferably 65-85°C, more preferably 70-80°C, such as 65°C, 70°C, 75°C, 80°C, 85°C, preferably a range value with the above arbitrary numerical value as the upper or lower limit; the reaction time is preferably 2-10 hours, more preferably 4-8 hours, such as 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, preferably a range value with the above arbitrary numerical value as the upper or lower limit.
[0046] After the reaction is completed, the reaction system is cooled to room temperature, solid-liquid separation is performed, and the obtained white solid is washed and dried to obtain polystyrene seed microspheres.
[0047] In the present invention, the solid-liquid separation can be high-speed centrifugal separation, and the centrifugal speed is preferably 4000-8000rpm, more preferably 5000-7000rpm, such as 4000rpm, 5000rpm, 6000rpm, 7000rpm, 8000rpm, preferably a range value with any of the above values as the upper or lower limit.
[0048] In the present invention, ethanol and deionized water are preferably used to wash the white solid obtained by solid-liquid separation in sequence; the present invention first uses ethanol to wash the white solid to remove the styrene monomer that does not participate in the reaction in the system, and then washes with water; if it is washed with water first, the residual styrene in the system is insoluble in water and tends to diffuse into the polystyrene seed microspheres. At this time, the polystyrene seed microspheres become larger due to the absorption of styrene monomers, thereby affecting the subsequent use of the seeds. The drying temperature is preferably 40 to 60°C, more preferably 50°C.
[0049] After the polystyrene seed microspheres are obtained, the present invention disperses them in deionized water, adds a dispersant and an emulsifier, and fully emulsifies them in an emulsifier to obtain a uniform emulsified solution of the polystyrene seed microspheres.
[0050] In the present invention, the dispersion may be carried out by at least one of mechanical stirring, magnetic stirring, ultrasonic wave, vortex and the like.
[0051] In the present invention, the dispersant is preferably one or more of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), and hydroxyethyl cellulose (HEC); the emulsifier is preferably one or more of sodium dodecyl sulfate (SDS), sodium dodecyl sulfonate (SLS), and sodium dodecylbenzene sulfonate (SDBS).
[0052] In the present invention, in the emulsified solution of polystyrene seed microspheres, the mass concentration of polystyrene seed microspheres is preferably 2-10 mg / mL, more preferably 3-9 mg / mL, such as 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL, 10 mg / mL, preferably a range value with any of the above numerical values as the upper or lower limit; the mass concentration of the dispersant is preferably 1-8 mg / mL, more preferably 3-5 mg / mL, such as 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, preferably a range value with any of the above numerical values as the upper or lower limit; the mass concentration of the emulsifier is preferably 0.2-5 mg / mL, more preferably 1-4 mg / mL, such as 0.2 mg / mL, 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, 3 The above range is preferably a range with any of the above values as the upper or lower limit.
[0053] The present invention has no special restrictions on the emulsification conditions of the emulsifier, and the emulsification process commonly used in the art can be adopted.
[0054] Then, the present invention dissolves the initiator into the styrene monomer and the divinylbenzene monomer (DVB), and adds the porogen, and mixes them thoroughly and evenly; then, the initiator is added into the polystyrene seed microsphere emulsified solution described above, and swells for 2 to 10 hours in an inert gas atmosphere, and then performs a polymerization reaction. After the reaction is completed, the solid-liquid separation is performed, and the obtained white solid is washed and dried to obtain monodispersed hollow polystyrene-divinylbenzene composite microspheres.
[0055] In the present invention, the initiator is one or more of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator and a redox system initiator, more preferably one or more of azobisisobutyronitrile (AIBN), dibenzoyl peroxide (BPO) and potassium persulfate; the porogen is preferably one or more of toluene, acetone and cyclohexane.
[0056] In the present invention, the ratio of the sum of the masses of the styrene monomer and the divinylbenzene monomer to the mass of the initiator is preferably (20-40):1, more preferably (25-35):1, such as 25:1, 30:1, 35:1, 40:1, preferably a range value with the above arbitrary numerical values as the upper or lower limit; the ratio of the sum of the masses of the styrene monomer and the divinylbenzene monomer to the mass of the porogen is preferably (1-5):(1-4), such as 1:1, 1:2, 1:3, 1:4, 2:1, 2:3, 3:1, 3:2, 3:4, 4:1, 4:3, 5:1, 5:2, 5:3, 5:4, preferably a range value with the above arbitrary numerical values as the upper or lower limit.
[0057] In the present invention, the swelling time is preferably 2 to 10 hours, more preferably 3 to 8 hours, such as 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, preferably a range value with any of the above values as the upper or lower limit.
[0058] The seed microspheres of 30000-40000 molecular weight used in the present invention have larger molecular weight, and the swelling time is shorter. The seed microspheres only swell in the peripheral part, and form a microreactor with monomers and porogens at the same time. When heated, the swollen microspheres preferentially react in the periphery, gradually forming a dense shell layer, and the unswollen seed part, monomers and porogens cannot enter, so they serve as templates. After a certain reaction time, the monomers are gradually consumed to form a complete shell layer, and the unparticipated toluene is squeezed to the inside due to the hydrophobic effect. Under high temperature conditions, toluene gradually dissolves the unswollen seed microspheres to form a linear polymer chain. After the reaction ends, it is removed together with toluene in the washing process, and finally forms a hollow structure. The amount of toluene is more, the part of the swollen seed is more, and the proportion of the unswollen seed is correspondingly less, and the finally formed cavity is small, otherwise, the formed cavity is large. If the swelling time is too long, porous structure is easily formed, and it is difficult to form a hollow structure. And through a large number of experiments of the present invention, it is verified that only when the molecular weight of the seed microspheres is between 30,000 and 40,000, a hollow structure can be formed. When the molecular weight is less than this, a porous structure is formed. When the molecular weight of the seed is too high, it is difficult to swell.
[0059] In the present invention, the inert gas is preferably one or more of nitrogen, helium and argon; the solid-liquid separation can be high-speed centrifugal separation, and the centrifugal speed is preferably 4000-8000rpm, more preferably 5000-7000rpm, such as 4000rpm, 5000rpm, 6000rpm, 7000rpm, 8000rpm, preferably a range value with any of the above values as the upper or lower limit.
[0060] In the present invention, ethanol and deionized water are preferably used to wash the white solid obtained by solid-liquid separation in sequence; the drying temperature is preferably 40-60°C, more preferably 50°C.
[0061] The present invention also provides a monodisperse hollow polystyrene-divinylbenzene composite microsphere, which is prepared according to the preparation method described above. In the present invention, the particle size of the monodisperse hollow polystyrene-divinylbenzene composite microsphere is preferably 1.5 to 3 μm.
[0062] The present invention also provides the use of the monodisperse hollow polystyrene-divinylbenzene composite microspheres as described above as a raw material for preparing chemiluminescent magnetic beads in enzyme-linked immunosorbent assay.
[0063] The present invention preferably deposits superparamagnetic ferroferric oxide nanoparticles inside and on the surface of the monodisperse hollow polystyrene-divinylbenzene composite microspheres described above, and wraps the polymer layer to prevent magnetic leakage; and modifies the surface with corresponding groups, such as amino, carboxyl, hydroxyl, carbonyl, thiol, etc., so that the chemiluminescent magnetic beads can be used in enzyme-linked immunosorbent assay. In the present invention, the particle size of the chemiluminescent magnetic beads is preferably 1.5 to 3 μm.
[0064] The specific steps are as follows:
[0065] 1) The monodisperse hollow polystyrene-divinylbenzene composite microspheres described above are mixed with sulfuric acid and nitric acid, and stirred to react to obtain nitrated microspheres.
[0066] In the present invention, the volume ratio of sulfuric acid to nitric acid is preferably (2-4):1, more preferably (2.5-3):1; the reaction temperature is preferably 25-35°C, more preferably 30°C; the reaction time is preferably 2-10 hours, more preferably 5-8 hours.
[0067] 2) Mixing the nitrated microspheres with a reducing agent to carry out a reduction reaction, reducing the nitro group to an amino group, and obtaining reduced microspheres.
[0068] In the present invention, the reducing agent is preferably a sulfide, more preferably one or more of sodium sulfide, sodium disulfide, sodium thiosulfate and sodium dithionite, the mass ratio of the nitrated microspheres to the reducing agent is preferably 1: (2-6), more preferably 1: (3-5), such as 1: 2, 1: 3, 1: 4, 1: 5, 1: 6, preferably a range value with any of the above values as the upper or lower limit. The temperature of the reduction reaction is preferably 60-80°C, more preferably 65-75°C, such as 60°C, 65°C, 70°C, 75°C, 85°C, preferably a range value with any of the above values as the upper or lower limit; the time of the reduction reaction is preferably 4-10 hours, more preferably 5-8 hours.
[0069] 3) Mixing the reduced microspheres with iron salt and alkali to react, depositing superparamagnetic ferroferric oxide nanoparticles inside and on the surface of the hollow microspheres, and obtaining magnetic hollow microspheres.
[0070] The iron salt preferably includes a divalent iron salt and a trivalent iron salt, and the molar ratio of the trivalent iron salt to the divalent iron salt is preferably 2:1; the base is preferably one or more of sodium hydroxide, potassium hydroxide and ammonia water, and the pH value of the reaction system in the present invention is preferably maintained at 9 to 11, more preferably 10, and the reaction time is preferably 2 to 8 hours, more preferably 3 to 5 hours. The reaction is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably one or more of helium, neon, argon and nitrogen.
[0071] 4) Mixing the magnetic hollow microspheres with monomers and initiators to react and wrap the surfaces of the magnetic hollow microspheres to form a complete shell layer.
[0072] In the present invention, the monomer is preferably a vinyl monomer, more preferably divinylbenzene and / or styrene, and the initiator is preferably one or more of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator and a redox system initiator, more preferably one or more of azobisisobutyronitrile (AIBN), dibenzoyl peroxide (BPO) and potassium persulfate.
[0073] In the present invention, the reaction temperature is preferably 60-80°C, more preferably 65-75°C, such as 60°C, 65°C, 70°C, 75°C, 85°C, preferably a range value with any of the above values as the upper or lower limit.
[0074] 5) Adding carboxyl-modified monomer and initiator to the encapsulated hollow microspheres prepared in step 4) above to react, thereby obtaining hollow spherical chemiluminescent magnetic beads.
[0075] In the present invention, the initiator is preferably one or more of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator and a redox system initiator, more preferably one or more of azobisisobutyronitrile (AIBN), dibenzoyl peroxide (BPO) and potassium persulfate; the carboxyl-modified monomer is preferably an acrylic compound, such as acrylic acid.
[0076] In the present invention, the reaction temperature is preferably 60-80°C, more preferably 65-75°C, such as 60°C, 65°C, 70°C, 75°C, 85°C, preferably a range value with any of the above values as the upper or lower limit; the reduction reaction time is preferably 4-10 hours, more preferably 5-8 hours.
[0077] Compared with the prior art, the present invention has the following advantages:
[0078] 1. The present invention first adopts a dispersion polymerization method to prepare polystyrene seed microspheres of different particle sizes and different molecular weights by adjusting the alcohol-water ratio, the amount of initiator and the dispersant, and uses the polystyrene seed microspheres as template balls, which are dispersed in the water phase, emulsified evenly, and the emulsified swelling agent, initiator and porogen are added. After swelling for a certain period of time, the reaction is directly carried out. The method is simple, time-saving and labor-saving, and can be prepared in batches;
[0079] 2. The process adds a certain amount of dispersant and uses ultrasound and mechanical stirring to assist synthesis, ensuring the monodispersity of the composite microspheres;
[0080] 3. By regulating relevant parameters, monodisperse hollow polystyrene-divinylbenzene composite microspheres with good stability, uniform particle size, adjustable particle size, controllable shell thickness, adjustable inner cavity size and easy surface modification can be prepared.
[0081] In order to further illustrate the present invention, a monodisperse hollow polystyrene-divinylbenzene composite microsphere provided by the present invention, its preparation method and application in enzyme-linked immunosorbent assay are described in detail below in conjunction with examples, but it should not be understood as limiting the scope of protection of the present invention.
[0082] Example 1
[0083] (1) 3 g of PVP was dissolved in a mixed solution of 40 ml of anhydrous ethanol and 100 ml of deionized water, and 10 ml of St and 0.5 g of AIBN were added. Nitrogen was introduced to deoxygenate and the system was maintained in a nitrogen atmosphere. Mechanical stirring was used to mix uniformly at a speed of 300 rpm. After reacting at 70 ° C for 3 h, it was naturally cooled to room temperature. The solid-liquid separation was performed by centrifugation at a speed of 8000 rpm. The obtained white solid was washed with ethanol and deionized water for several times, and then dried at 50 ° C to obtain polystyrene seed microspheres;
[0084] (2) dispersing 0.5 g of the polystyrene seed microspheres obtained in step (1) into 200 ml of deionized water, adding 0.2 g of SDS emulsifier, and fully emulsifying with an emulsifier to obtain a uniform emulsified solution containing the polystyrene seed microspheres;
[0085] (3) Dissolve 0.7g AIBN initiator in 10ml St and 10ml DVB, add 10ml toluene, mix well by mechanical stirring, set the speed at 300rpm; add it to the emulsion in step (2), introduce nitrogen, swell for 10h, add 1g PVP dispersant. Under 70℃, mechanical stirring, set the speed at 300rpm, react for 8h, separate solid and liquid by centrifugation, set the centrifugal speed at 8000rpm, wash the obtained white solid with ethanol and deionized water several times, and then dry it at 50℃ to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres;
[0086] The appearance of the polystyrene seed microspheres and composite microspheres prepared in Example 1 is as follows: Figure 1 As shown in the figure, they are milky white, and have good suspension and high dispersibility in aqueous solution. Figure 2 As shown in the figure, it can be seen that the seed microspheres have good monodispersity. The particle size distribution diagram of the polystyrene seed microspheres prepared in Example 1 is shown in Figure 3 As shown by Figure 3It can be seen that the seed microspheres have a narrow particle size distribution; the microscopic photograph of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1 is shown in FIG. Figure 4 As shown in the figure, it can be seen that the microspheres are hollow structures. The scanning electron microscope photo of the polystyrene seed microspheres prepared in Example 1 is shown in Figure 5 As shown in the figure, it can be seen that the prepared polystyrene seed microspheres have good monodispersity and uniform particle size, with a size of about 800nm; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1 is shown in Figure 6 As shown in the figure, it can be seen that the composite microspheres have good monodispersity, a smooth surface, no defects, uniform particle size, and a size of about 1.9 μm; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1 after grinding is shown in Figure 7 As shown in the figure, it can be seen that after the composite microspheres are crushed, the inside is a hollow structure, and the shell thickness is about 220nm;
[0087] Example 2
[0088] (1) 4 g of PVP was dissolved in a mixed solution of 40 ml of anhydrous ethanol and 110 ml of deionized water, and 10 ml of St and 0.6 g of AIBN were added. Nitrogen was introduced to deoxygenate and the system was maintained in a nitrogen atmosphere. Mechanical stirring was used to mix uniformly at a speed of 300 rpm. After reacting at 70 ° C for 5 h, it was naturally cooled to room temperature. The solid-liquid separation was performed by centrifugation at a speed of 8000 rpm. The obtained white solid was washed with ethanol and deionized water for several times, and then dried at 50 ° C to obtain polystyrene seed microspheres;
[0089] (2) dispersing 0.5 g of the polystyrene seed microspheres obtained in step (1) into 200 ml of deionized water, adding 1 g of PVP dispersant and 0.2 g of SDS emulsifier, and fully emulsifying with an emulsifier to obtain a uniform emulsified solution containing polystyrene seed microspheres;
[0090] (3) Dissolve 0.7 g of AIBN initiator in 10 ml of St and 10 ml of DVB, add 20 ml of toluene, mix well by mechanical stirring, and set the speed at 300 rpm; add the mixture to the emulsion in step (2), introduce nitrogen, swell for 8 h, mechanically stir at 75 ° C, set the speed at 300 rpm, react for 8 h, separate the solid and liquid by centrifugation, set the centrifugal speed at 8000 rpm, wash the obtained white solid with ethanol and deionized water several times, and then dry at 50 ° C to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres;
[0091] The scanning electron microscope photo of the polystyrene seed microspheres prepared in Example 2 is as follows: Figure 8 As shown in the figure, it can be seen that the prepared polystyrene seed microspheres have good monodispersity and uniform particle size, with a size of about 700nm; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 2 is shown in Fig. 9 As shown in the figure, it can be seen that the composite microspheres have good monodispersity, smooth surface, no defects, and uniform particle size; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 2 after grinding is shown in Fig.10 As shown in the figure, it can be seen that after the composite microspheres are crushed, the interior is a hollow structure with a shell thickness of about 420nm. Increasing the amount of porogen toluene increases the proportion of swollen seeds, the particle size of the remaining unswollen seeds is smaller, and the inner cavity is correspondingly reduced.
[0092] Example 3
[0093] (1) 2 g of PVP was dissolved in a mixed solution of 40 ml of anhydrous ethanol and 110 ml of deionized water, and 10 ml of St and 0.6 g of AIBN were added. Nitrogen was introduced to deoxygenate and the system was maintained in a nitrogen atmosphere. Mechanical stirring was used to mix uniformly at a speed of 300 rpm. After reacting at 70 ° C for 3 h, it was naturally cooled to room temperature. The solid-liquid separation was performed by centrifugation at a speed of 8000 rpm. The obtained white solid was washed with ethanol and deionized water for several times, and then dried at 50 ° C to obtain polystyrene seed microspheres;
[0094] (2) dispersing 0.5 g of the polystyrene seed microspheres obtained in step (1) into 200 ml of deionized water, adding 1 g of PVP dispersant and 0.2 g of SDS emulsifier, and fully emulsifying with an emulsifier to obtain a uniform emulsified solution containing polystyrene seed microspheres;
[0095] (3) Dissolve 0.7 g of AIBN initiator in 10 ml of St and 10 ml of DVB, add 5 ml of toluene, mix well by mechanical stirring, and set the speed at 300 rpm; add the mixture to the emulsion in step (2), introduce nitrogen, swell for 8 h, mechanically stir at 75 ° C, set the speed at 300 rpm, react for 8 h, separate the solid and liquid by centrifugation, set the centrifugal speed at 8000 rpm, wash the obtained white solid with ethanol and deionized water several times, and then dry at 50 ° C to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres;
[0096] The scanning electron microscope photo of the polystyrene seed microspheres prepared in Example 3 is as follows: Fig.11As shown in the figure, it can be seen that the prepared polystyrene seed microspheres have good monodispersity and uniform particle size, about 900nm, and the particle size of the seed microspheres can be regulated by adjusting the proportion of PVP; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 3 is shown in Fig.12 As shown in the figure, it can be seen that the composite microspheres have good monodispersity, a smooth surface, no defects, and uniform particle size; the scanning electron microscope photo of the monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 3 after grinding is shown in Fig.13 As shown in the figure, it can be seen that after the composite microspheres are crushed, the interior is a hollow structure with a shell thickness of about 190nm. As the proportion of the porogen increases, the shell thickness of the microspheres increases.
[0097] It can be seen from the above embodiments that the present invention can control the size of polystyrene seed microspheres by adjusting the amount of PVP; and control the shell thickness and inner cavity size of the composite microspheres by controlling the amount of porogen toluene, thereby controlling the overall structure and morphology of the composite microspheres.
[0098] Application Examples
[0099] (1) The monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared in Example 1 were subjected to nitration reaction: a certain amount of sulfuric acid and nitric acid (volume ratio of 2.5:1) were poured into a four-necked flask and placed in ice water, 2 g of polystyrene-divinylbenzene composite microspheres were added dropwise, and the reaction was stirred at 30° C. for 6 h. After the reaction was completed, nitrated microspheres were obtained, which were washed with deionized water until neutral and set aside.
[0100] (2) Reducing the nitro groups on the nitrated microspheres to amino groups: First, the nitrated microspheres were dispersed in a certain volume of deionized water, and the reducing agent sodium dithionite was added. The mass ratio of the nitrated microspheres to the reducing agent was 1:4. The reaction was carried out at a reaction temperature of 70°C for 6 hours. After the reaction was completed, the microspheres were washed several times with deionized water for later use.
[0101] (3) Magnetic deposition: After the hollow polystyrene-divinylbenzene composite microspheres were modified by amino, a certain amount of Fe was adsorbed. 3+ / Fe 2+ The ratio of the two is 2:1, and a certain amount of ammonia water is added to maintain the pH of the whole system at 10. The reaction is carried out for 4 hours. After the reaction is completed, magnetic hollow microspheres are obtained. The whole process is carried out in an inert gas atmosphere.
[0102] (4) Surface coating: Surface coating of the magnetic hollow microspheres is performed to prevent the magnetic particles from falling off and being oxidized. Specific steps: Take the magnetic hollow microspheres, add vinyl monomer (DVB:St=5:1), and add initiator AIBN, and coat at 70°C to form a complete shell layer.
[0103] (5) Carboxylation modification: Take the above-mentioned encapsulated hollow magnetic microspheres, add acrylic acid and initiator AIBN, and react at 70° C. for 6 hours to finally obtain carboxylated hollow magnetic beads.
[0104] The scanning electron microscope image of the prepared carboxylated hollow magnetic beads is shown in Fig.14 As shown in the figure, it can be seen that a large number of magnetic particles are attached to the surface of the magnetic beads, and the magnetic particles do not fall off, indicating that the prepared carboxylation hollow magnetic beads have good stability; the carboxylation magnetic beads are in a monodisperse state, which increases the specific surface area of the magnetic beads, and the raised magnetic particles on the surface further increase the specific surface area of the magnetic beads, providing more binding sites in the enzyme-linked immunosorbent assay, which is beneficial to increase the signal value of the sample to be tested, thereby reducing the detection limit of the sample to be tested.
[0105] Table 1 Evaluation of the application of prepared carboxylated magnetic beads in the tumor marker (cyfra21-1) project
[0106]
[0107]
[0108] Table 1 shows that after magnetic beads were coated, they had higher signal values and less passive adsorption, indicating that hollow magnetic beads have great application prospects in enzyme-linked immunosorbent assays.
[0109] The responsiveness of carboxylated hollow magnetic beads was detected using an absorbance instrument. The results are as follows: Fig.15 As shown by Fig.15 It can be seen that within 10 seconds, the magnet absorbs 75% of the magnetic beads, within 20 seconds, 95% of the magnetic beads, and within 30 seconds, 100% of the magnetic beads. This shows that the carboxylated hollow magnetic beads prepared by the present invention have strong magnetism and short magnetic response time.
[0110] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing monodisperse hollow polystyrene-divinylbenzene composite microspheres, comprising the following steps: A) mixing polystyrene seed microspheres with a molecular weight of 30,000 to 40,000, a dispersant and an emulsifier, and emulsifying to obtain an emulsified solution of polystyrene seed microspheres; In the emulsified solution of polystyrene seed microspheres, the mass concentration of the polystyrene seed microspheres is 2 to 10 mg / mL; the mass concentration of the dispersant is 1 to 8 mg / mL; and the mass concentration of the emulsifier is 0.2 to 5 mg / mL; B) mixing an initiator, a styrene monomer, a divinylbenzene monomer and a porogen uniformly, adding the mixture to the emulsified solution of the polystyrene seed microspheres, and performing a polymerization reaction after swelling for 2 to 10 hours under an inert gas atmosphere, washing and drying the obtained product to obtain monodisperse hollow polystyrene-divinylbenzene composite microspheres; The ratio of the sum of the mass of the styrene monomer and the divinylbenzene monomer in step B) to the mass of the initiator in step B) is (20-40):1; the ratio of the sum of the mass of the styrene monomer and the divinylbenzene monomer in step B) to the mass of the porogen is (1-5):(1-4).
2. The preparation method according to claim 1, characterized in that: The polystyrene seed microspheres are prepared according to the following steps: Adding polyvinyl pyrrolidone, styrene monomer and initiator into an alcohol-water mixed solution, reacting at 65-85° C. for 2-10 hours in an inert gas atmosphere to obtain polystyrene seed microspheres; The initiator is one or more of an azo initiator, an organic peroxide initiator, and an inorganic peroxide initiator.
3. The preparation method according to claim 2, characterized in that: The mass ratio of alcohol to water in the alcohol-water mixed solution is (2-4):1; the molar ratio of the styrene monomer to the initiator is (10-20):1; and the mass ratio of the polyvinyl pyrrolidone to the styrene monomer is 1:(3-8).
4. The preparation method according to claim 1, characterized in that: In the step A), the dispersant is one or more of polyvinyl pyrrolidone, polyvinyl alcohol, and hydroxyethyl cellulose; and the emulsifier is one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
5. The preparation method according to claim 1, characterized in that: The initiator in step B) is one or more of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator and a redox system initiator; The porogen in step B) is one or more of toluene, acetone and cyclohexane.
6. The preparation method according to claim 1, characterized in that: The polymerization reaction temperature in step B) is 65-85° C. and the polymerization reaction time is 5-10 hours.
7. Monodisperse hollow polystyrene-divinylbenzene composite microspheres prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the monodisperse hollow polystyrene-divinylbenzene composite microspheres as claimed in claim 7 in enzyme-linked immunosorbent assay.
9. The use according to claim 8, characterized in that: The monodisperse hollow polystyrene-divinylbenzene composite microspheres are sequentially subjected to nitration, reduction, magnetic deposition of superparamagnetic ferroferric oxide nanoparticles, coating with a polymer layer and surface carboxylation modification to obtain hollow spherical chemiluminescent magnetic beads, which are applied to enzyme-linked immunosorbent assay.