A railway rail under-rail elastic pad and its preparation method

By adjusting the component ratio of polyols and prepolymers, a polyurethane elastic pad with high static stiffness and low compression permanent deformation was prepared, which solved the shortcomings of the existing elastic pad under the rail in terms of load-bearing capacity and durability, and achieved the Higher railway track load-bearing capacity and longer service life.

CN115677960BActive Publication Date: 2024-11-19BEIJING COMENS NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211430633.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-15
Publication Date
2024-11-19
Estimated Expiration
2042-11-15

AI Technical Summary

Technical Problem

The existing elastic pads under railway tracks have shortcomings in terms of dynamic-static ratio, large compression permanent deformation and durability, which affects the stability and load-bearing capacity of the train.

Method used

Polyurethane elastic pads made of polyol A component and prepolymer B component are made of 1:1 to 2.5 mass ratio. By adjusting the ratio of soft and hard segments, the type and proportion of chain extenders, the static stiffness and resistance are improved. Fatigue performance, reducing compression permanent deformation.

Benefits of technology

It significantly improves the load-bearing capacity and service life of railway tracks, with a static stiffness of 90~120KN/mm, a permanent compression deformation of only 5%, and a dynamic-static ratio of less than 1.5, and has excellent aging resistance and fatigue resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005012964000000011
    Figure FDA0005012964000000011
  • Figure GDA0005012964010000021
    Figure GDA0005012964010000021
  • Figure GDA0005012964010000041
    Figure GDA0005012964010000041
Patent Text Reader

Abstract

The invention discloses an elastic pad under rail for railway and a preparation method thereof. The raw materials of the elastic pad are measured by mass. 40-60 parts of polyether polyol and 40-60 parts of isocyanate are reacted at 70-90°C to obtain a prepolymer B component; 50-80 parts of polyether polyol, 10-30 parts of chain extender, 3-8 parts of cross-linking agent, 0.1-1 part of catalyst, 0.5-1 part of foam stabilizer, 0.5-2 parts of stabilizer, and 0.05-0.2 parts of water are mixed evenly to obtain a polyol A component; the polyol A component and the prepolymer B component are mixed at a mass ratio of 1:1-2.5, injected into a mold, and the mold is placed in a 70-120°C condition for further reaction and aging for 8-30 minutes, and then removed from the mold and placed in a constant temperature room or 100°C for aging for 12-24 hours to obtain an elastic pad that meets the standards of the Institute of Railway Science. The elastic pad has excellent tensile properties, low compression permanent deformation, and good fatigue resistance. When pouring through a two-component polyurethane pouring machine, the molding time is short, which greatly improves production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new chemical materials, specifically to an elastic pad for railway rails and its preparation method. Background Technology

[0002] The elastic pad under the rail for railway tracks is an important component of the track structure. It is installed between the steel rail and the concrete sleeper. Its main function is to buffer the high-frequency vibration and impact generated during vehicle operation, protect the roadbed and sleeper, and in special cases, such as subways and high-speed railways, it also plays a role in reducing noise.

[0003] Currently, commonly used materials for rail under-track elastic pads include EPDM, SBR, natural rubber, polyester elastomers, and polyurethane. EPDM, SBR, and natural rubber, however, have drawbacks such as a high dynamic-to-static ratio, large compression set, and poor durability, which can affect the smoothness of train operation. Polyester elastomers possess excellent mechanical properties and fatigue resistance, but their hydrolytic resistance is poor and their cost is high. Compared to the above materials, polyurethane elastomers have relatively better mechanical properties, better fatigue resistance than rubber, and are close to those of polyester elastomers. Their durability is better than both rubber and polyester elastomers, and their cost is more moderate, making them widely used in cushioning and vibration damping products.

[0004] Chinese patent application CN102618038A discloses a method for preparing an elastic track pad by using methyl vinyl silicone rubber as the main material and adding reinforcing agents, structure control agents, vulcanizing agents, etc., and then vulcanizing it at high temperature. However, the elastic track pad prepared by this patent application has low strength and high compression set.

[0005] Chinese patent application CN105619739A discloses a method for preparing a heavy-duty railway elastic pad by mixing TPEE modified material with nucleating agent, antioxidant, polycarbonimide and UV stabilizer in a certain proportion and then molding it through injection molding. The elastic pad prepared by this patent application has high tensile strength and elongation at break, but its process is relatively complex and costly.

[0006] Chinese patent application CN108559252A discloses the preparation of an elastic pad for derailment by adding modified cork particles to a polyurethane composite. However, the test results do not specify data such as compression set and dynamic-to-static ratio. Furthermore, this patent application is for a three-component polyurethane, which involves a relatively complex process.

[0007] Therefore, in order to improve the smoothness and load-bearing capacity of train operation, it is a problem that needs to be solved to provide an elastic pad with higher overall performance.

[0008] In view of this, the present invention is hereby proposed. Summary of the Invention

[0009] In view of the above-mentioned shortcomings in the prior art, the present invention provides a railway under-rail elastic pad and its preparation method, which has high load-bearing capacity and long service life, and can well meet the requirements of railway track under-rail elasticity and durability.

[0010] The purpose of this invention is to provide a technical solution as follows:

[0011] A type of elastic track pad for railways is made by combining polyol component A and prepolymer component B in a mass ratio of 1:1 to 2.5; wherein, the polyol component A is made from the following raw materials in parts by mass:

[0012]

[0013] The prepolymer component B is made from the following raw materials in parts by mass:

[0014] 40-60 parts of polyether diol

[0015] 40-60 parts of isocyanate.

[0016] A method for preparing a railway rail under-rail elastic pad according to the present invention includes the following steps:

[0017] Polyol component A and prepolymer component B were prepared separately; wherein,

[0018] According to the formulation of the polyol A component of the railway rail elastic pad described in this invention, the raw materials are taken, and the preparation of the polyol A component includes:

[0019] The polyether diol, polyether polyol, chain extender, crosslinking agent, stabilizer, and foam stabilizer are added to the reactor and stirred at 40-90°C. After mixing evenly, the moisture content is tested. Then, the pigment, foaming agent, and catalyst are added to the reactor and mixed evenly. The mixture is then discharged, sealed, and stored.

[0020] According to the formulation of the prepolymer B component of the railway rail under-rail elastic pad of the present invention, the raw materials are taken, and the preparation of the prepolymer B component includes:

[0021] The polyether polyol and isocyanate were reacted at 70-90°C for 2 hours. The NCO content was tested. After passing the test, the material was discharged and sealed for storage.

[0022] After the material temperature is constant at 30-80℃, the polyol component A and prepolymer component B prepared above are mixed evenly at a mass ratio of 1:1-2.5 and then injected into the mold of the rail elastic pad. The temperature of the rail elastic pad mold is 60-120℃. After 8-30 minutes, the material is removed from the mold and placed in a constant temperature room or at 100℃ for 12-24 hours to mature, thus obtaining the rail elastic pad for railway use.

[0023] The beneficial effects of this invention are as follows: The railway rail under-rail elastic pad prepared by this invention is a polyurethane elastic pad. By adjusting the ratio of soft and hard sections, the type and ratio of chain extender, and the type of soft section, its static stiffness reaches 90-120 KN / mm, greatly improving the load-bearing capacity of the railway. This railway rail under-rail elastic pad has excellent tensile strength and elongation at break. The tensile strength can reach 17 MPa, and the elongation at break is greater than 400%. The compression set of this railway rail under-rail elastic pad is only 5%, and the dynamic-to-static ratio is less than 1.5. The elastic pad does not break after 3 million load cycles, and the static stiffness change rate of the elastic pad is less than 10%. This railway rail under-rail elastic pad has excellent aging resistance, with a tensile strength of 12-15 MPa and an elongation of 390-450% after aging. In summary, the elastic pad prepared by this invention has high load-bearing capacity and long service life. Detailed Implementation

[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them, and do not constitute a limitation on the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the protection scope of the present invention.

[0025] First, the following explanations are provided for the terms that may be used in this article:

[0026] The terms “including,” “comprising,” “containing,” “having,” or other similar semantic descriptions shall be interpreted as non-exclusive inclusion. For example, “including a technical feature element (such as raw material, component, ingredient, carrier, dosage form, material, size, part, component, mechanism, device, step, process, method, reaction conditions, processing conditions, parameter, algorithm, signal, data, product or article of manufacture, etc.)” shall be interpreted as including not only the expressly listed technical feature element, but also other technical feature elements known in the art that are not expressly listed.

[0027] The term "parts by weight" indicates the mass ratio between multiple components. For example, if component X is described as x parts by weight and component Y as y parts by weight, then the mass ratio of component X to component Y is x:y. One part by weight can represent any mass; for example, one part by weight can be expressed as 1 kg or 3.1415926 kg, etc. The sum of the parts by weight of all components is not necessarily 100 parts; it can be greater than 100 parts, less than 100 parts, or equal to 100 parts. Unless otherwise stated, parts, proportions, and percentages mentioned herein are all by mass.

[0028] When concentration, temperature, pressure, size, or other parameters are expressed as numerical ranges, such ranges should be understood to specifically disclose all ranges formed by any pairing of upper limits, lower limits, or preferred values ​​within that range, regardless of whether the range is explicitly stated; for example, if the numerical range "2 to 8" is stated, then that range should be interpreted to include ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise stated, the numerical ranges described herein include both their endpoints and all integers and fractions within that range.

[0029] The following is a detailed description of the railway rail elastic pad and its preparation method provided by the present invention. Contents not described in detail in the embodiments of the present invention are prior art known to those skilled in the art. Where specific conditions are not specified in the embodiments of the present invention, they shall be performed according to conventional conditions in the art or conditions recommended by the manufacturer. Reagents or instruments used in the present invention whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0030] The following is a detailed description of an elastic track pad for railways and its preparation method provided by the present invention. Contents not described in detail in the embodiments of the present invention are prior art known to those skilled in the art.

[0031] This invention provides a railway rail under-rail elastic pad, which is made of polyol component A and prepolymer component B in a mass ratio of 1:1 to 2.5. The polyol component A, by mass, includes the following raw materials:

[0032]

[0033] The prepolymer component B, by mass, comprises the following raw materials:

[0034] Polyether diol 40-60

[0035] Isocyanate 40-60

[0036] As a preferred embodiment, the polyether diol in component A is one or more of polytetrahydrofuran diol, tetrahydrofuran-propylene oxide co-ether diol, etc., with a molecular weight of 1000 to 3000.

[0037] As a preferred embodiment, the polyether polyol in polyol component A is one or more of polyoxypropylene triol, polyethylene oxide propylene triol, polytetrahydrofuran triol, tetrahydrofuran-propylene oxide co-ether triol, etc., with a molecular weight of 2000 to 6000.

[0038] As a preferred embodiment, the chain extender in polyol A component is a small molecule diamine and a small molecule diol.

[0039] As a preferred embodiment, the crosslinking agent in the polyol A component is one or more of low molecular weight polyether polyol, trimethylolpropane, triethanolamine, triisopropanolamine, glycerol, etc.

[0040] In a preferred embodiment of the railway track under-rail elastic pad described in this invention, the stabilizer in the polyol A component is a light stabilizer and an antioxidant.

[0041] As a preferred embodiment, the foam stabilizer in polyol A component is an organosilicon foam stabilizer.

[0042] As a preferred embodiment, the pigment in the polyol A component includes any one of color paste or powder pigment.

[0043] As a preferred embodiment, the foaming agent in polyol component A is water. Using water as the foaming agent eliminates the generation of harmful gases during the preparation process, making it environmentally friendly.

[0044] As a preferred embodiment, the catalyst in polyol A is an amine catalyst or an organotin catalyst, including but not limited to triethylenediamine, dibutyltin dilaurate, stannous octoate, etc.

[0045] As a preferred embodiment, the polyether diol in prepolymer component B is one or more of polytetrahydrofuran diol and tetrahydrofuran-propylene oxide coether diol.

[0046] As a preferred embodiment, the isocyanate in prepolymer component B is one or more of toluene diisocyanate, diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate.

[0047] This invention also provides a method for preparing the above-mentioned railway track elastic pad, which can produce a polyurethane elastic pad that meets the standards. The preparation method includes:

[0048] Polyol component A and prepolymer component B were prepared separately; wherein,

[0049] Take the raw materials for polyol A according to the above formula, and prepare polyol A according to the following steps:

[0050] The polyether diol, polyether polyol, chain extender, crosslinking agent, stabilizer, and foam stabilizer are added to the reactor and stirred at 40-90°C. After mixing evenly, the moisture content is tested. Then, the pigment, foaming agent, and catalyst are added to the reactor and mixed evenly. The mixture is then discharged, sealed, and stored.

[0051] Take the raw materials of polyol A component according to the above formula, and prepare prepolymer B component according to the following steps:

[0052] The polyether polyol and isocyanate were reacted at 70-90°C for 2 hours. The NCO content was tested. After passing the test, the material was discharged and sealed for storage.

[0053] After the material temperature stabilizes at 30–80°C, the polyol component A and prepolymer component B prepared above are mixed evenly at a mass ratio of 1:1–2.5 and then injected into the mold for the rail elastic pad. The mold temperature is 60–120°C. After 8–30 minutes, the mixture is removed from the mold and placed in a constant temperature chamber or at 100°C for 12–24 hours to obtain the railway rail elastic pad. Specifically, after the material temperature stabilizes (30–80°C), metering begins. The polyol component A and prepolymer component B prepared above are combined and injected into the casting machine at a mass ratio of 1:1–2.5. After being mixed evenly by the casting machine head, the mixture is injected into the mold. The mold temperature is 60–120°C. After 8–30 minutes, the mixture is removed from the mold and placed in a constant temperature chamber or at 100°C for 12–24 hours to obtain the railway rail elastic pad that meets the standards of the China Academy of Railway Sciences.

[0054] The polyurethane elastic pad prepared by the above preparation method has the following characteristics: (1) high tensile strength and elongation at break; (2) excellent fatigue resistance; (3) low dynamic-to-static ratio; (4) low compression set; and (5) excellent oil resistance and aging resistance.

[0055] To more clearly demonstrate the technical solution and its effects provided by the present invention, the following detailed description of the railway rail elastic pad and its preparation method provided by the present invention is based on specific embodiments.

[0056] Example 1

[0057] This embodiment provides a railway rail under-rail elastic pad and its preparation method, including the following steps:

[0058] Preparation of polyol component A:

[0059] 15.5 kg of polytetrahydrofuran glycol, 2.01 kg of polypropylene oxide triol, 1.5 kg of ethylene glycol, 0.5 kg of polypropylene oxide triol, 0.18 kg of foaming agent, and 0.13 kg of antioxidant were added to the reactor. The reactor temperature was controlled at 45℃. After stirring for 30 minutes, the water content was tested, and water was added to bring the total to 800 ppm. Then, 0.03 kg of organotin catalyst, 0.15 kg of triethylenediamine, and 0.15 kg of pigment were added. The mixture was stirred for 40 minutes, then discharged and sealed for storage.

[0060] Preparation of prepolymer component B:

[0061] 20 kg of polytetrahydrofuran diol was added to the reactor, along with 18 kg of diphenylmethane diisocyanate. The temperature was then raised to 80°C and reacted for 2 hours. The NCO content was tested, and if it passed the test, the material was discharged and sealed for storage.

[0062] Polyol component A and prepolymer component B are injected into the casting machine. After the material temperature stabilizes (40℃), metering begins. The mass ratio of polyol component A to prepolymer component B is 1:1.4. After the polyol component A and prepolymer component B are evenly mixed by the casting machine head, they are injected into the mold. The mold temperature is 70℃. After 12 minutes, the mixture is removed from the mold to obtain the elastic pad for railway rails.

[0063] Example 2

[0064] This embodiment provides a railway rail under-rail elastic pad and its preparation method, including the following steps:

[0065] Preparation of polyol component A:

[0066] 20 kg of polytetrahydrofuran-propylene oxide copolyether diol, 1.5 kg of polypropylene oxide ethylene oxide copolyether triol, 2.8 kg of 1,4-butanediol, 0.5 kg of polypropylene oxide triol, 0.2 kg of foaming agent, and 0.15 kg of antioxidant were added to the reactor. The reactor temperature was controlled at 45℃. After stirring for 30 minutes, the water content was tested, and water was added to bring the total to 800 ppm. Then, 0.04 kg of organotin catalyst and 0.18 kg of pigment were added, and the mixture was stirred for 40 minutes before being discharged and sealed for storage.

[0067] Preparation of prepolymer component B:

[0068] 25 kg of polytetrahydrofuran diol was added to the reactor, along with 30 kg of diphenylmethane diisocyanate. The temperature was then raised to 80°C and reacted for 2 hours. The NCO content was tested, and if it passed the test, the material was discharged and sealed for storage.

[0069] Polyol component A and prepolymer component B are injected into the casting machine. After the material temperature stabilizes (40℃), metering begins. The mass ratio of polyol component A to prepolymer component B is 1:1.4. After the polyol component A and prepolymer component B are evenly mixed by the casting machine head, they are injected into the mold. The mold temperature is 70℃. After 12 minutes, the mixture is removed from the mold to obtain the elastic pad for railway rails.

[0070] Example 3

[0071] This embodiment provides a railway rail under-rail elastic pad and its preparation method, including the following steps:

[0072] Preparation of polyol component A:

[0073] 20 kg of polytetrahydrofuran glycol, 2.5 kg of polyoxypropylene oxide ethylene oxide copolyether triol, 2.5 kg of 1,4-butanediol, 0.5 kg of 4,4'-methylenedi(2-chloroaniline), 0.5 kg of trimethylolpropane, 0.2 kg of foaming agent, and 0.15 kg of antioxidant were added to a reactor. The reactor temperature was controlled at 90℃. After stirring until 4,4'-methylenedi(2-chloroaniline) dissolved, the mixture was stirred for 30 minutes and then cooled down to 60℃. The water content was tested, and water was added to bring the total water content to 1000 ppm. Then, 0.04 kg of organotin catalyst and 0.18 kg of pigment were added. The mixture was stirred and mixed for 40 minutes before being discharged and sealed for storage.

[0074] Preparation of prepolymer component B:

[0075] 20 kg of polytetrahydrofuran-propylene oxide copolyether diol was added to the reactor, along with 25 kg of diphenylmethane diisocyanate. The temperature was then raised to 80°C and reacted for 2 hours. The NCO content was tested, and if it passed the test, the material was discharged and sealed for storage.

[0076] Polyol component A and prepolymer component B are injected into the casting machine. After the material temperature stabilizes (40℃), metering begins. The mass ratio of polyol component A to prepolymer component B is 1:1.4. After the polyol component A and prepolymer component B are evenly mixed by the casting machine head, they are injected into the mold. The mold temperature is 90℃. After 25 minutes, the mixture is removed from the mold. The elastic pad is then placed in a 100℃ oven for 12 hours to cure, resulting in the elastic pad for railway rails.

[0077] Example 4

[0078] This embodiment provides a railway rail under-rail elastic pad and its preparation method, including the following steps:

[0079] Preparation of polyol component A:

[0080] 20 kg of polytetrahydrofuran glycol, 1.9 kg of polyoxypropylene oxide ethylene oxide copolyether triol, 1 kg of ethylene glycol, 1 kg of 1,4-butanediol, 1 kg of 1,6-hexanediol, 0.2 kg of trimethylolpropane, 0.2 kg of foaming agent, and 0.15 kg of antioxidant were added to a reactor. The reactor temperature was controlled at 60℃. After stirring for 30 minutes, the water content was tested, and water was added to bring the total to 1500 ppm. Then, 0.04 kg of organotin catalyst, 0.15 kg of N-methylmorpholine, and 0.18 kg of pigment were added. The mixture was stirred for 40 minutes, then discharged and sealed for storage.

[0081] Preparation of prepolymer component B:

[0082] 20 kg of polytetrahydrofuran diol was added to the reactor, along with 18 kg of diphenylmethane diisocyanate. The temperature was then raised to 80°C and reacted for 2 hours. The NCO content was tested, and if it passed the test, the material was discharged and sealed for storage.

[0083] Polyol component A and prepolymer component B are injected into the casting machine. After the material temperature stabilizes (40℃), metering begins. The mass ratio of polyol component A to prepolymer component B is 1:2.5. After the polyol component A and prepolymer component B are evenly mixed by the casting machine head, they are injected into the mold. The mold temperature is 70℃. After 12 minutes, the mixture is removed from the mold to obtain the elastic pad for railway rails.

[0084] Example 5

[0085] This embodiment provides a railway rail under-rail elastic pad and its preparation method, including the following steps:

[0086] Preparation of polyol component A:

[0087] 25 kg of polytetrahydrofuran glycol, 1.8 kg of polytetrahydrofuran-propylene oxide copolyether triol, 3 kg of 1,4-butanediol, 1 kg of low molecular weight polyoxypropylene oxide triol, 0.24 kg of foaming agent, and 0.17 kg of antioxidant were added to a reactor. The reactor temperature was controlled at 45℃. After stirring for 30 minutes, the water content was tested, and water was added to bring the total to 1000 ppm. Then, 0.05 kg of organotin catalyst, 0.20 kg of tetramethylbutanediamine, and 0.20 kg of pigment were added. The mixture was stirred for 40 minutes, then discharged and sealed for storage.

[0088] Preparation of prepolymer component B:

[0089] Add 20 kg of polytetrahydrofuran diol to the reactor, add 20 kg of diphenylmethane diisocyanate, then heat to 80°C and react for 2 hours. Test the NCO content, and after passing the test, discharge the material and seal it for storage.

[0090] Polyol component A and prepolymer component B are injected into the casting machine. After the material temperature stabilizes (40℃), metering begins. The mass ratio of polyol component A to prepolymer component B is 1:1.3. After the polyol component A and prepolymer component B are evenly mixed by the casting machine head, they are injected into the mold. The mold temperature is 90℃. After 12 minutes, the mixture is removed from the mold and then placed in a 100℃ oven for 12 hours to obtain the elastic pad for railway rails.

[0091] Comparative Example

[0092] Elastic pads produced by a railway parts company.

[0093] The track-mounted elastic pads of Examples 1-5 and the comparative examples were subjected to performance testing. The specific testing methods are as follows:

[0094] (1) Mechanical properties: The tensile strength and elongation at break of the body were tested in accordance with GB / T 10654-2001;

[0095] (2) Compression set: The test conditions were 70℃, 22h, and 30% compression.

[0096] (3) Static stiffness and dynamic-to-static ratio: Refer to the general technical conditions for fasteners of high-speed railways;

[0097] (4) Aging conditions: 70℃, 168h.

[0098] Performance tests are shown in Table 1.

[0099]

[0100]

[0101] The comparison in the table above shows that the polyurethane-type railway rail elastic pad prepared by this invention, through adjusting the ratio of hard and soft sections, the type and ratio of chain extender, and the type of soft section, achieves a static stiffness of 90–120 KN / mm, greatly improving the load-bearing capacity of the railway. It exhibits excellent tensile strength and elongation at break, with a tensile strength reaching 17 MPa, an elongation at break greater than 400%, and a compression set of only 5%, resulting in a dynamic-to-static ratio below 1.5. The elastic pad shows no damage after 3 million load cycles, and the static stiffness change rate is less than 10%. It also demonstrates excellent aging resistance, with a tensile strength of 12–15 MPa and an elongation of 390–450% after aging. Compared to the comparative example, the rail elastic pad prepared by this invention has significant advantages in elongation at break and compression set, and the low compression set is beneficial to the smoothness of train operation.

[0102] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims. The information disclosed in the background section is intended only to enhance the understanding of the overall background technology of the present invention and should not be construed as an admission or implication in any way that such information constitutes prior art known to those skilled in the art.

Claims

1. A railway rail elastic pad, characterized in that: The polyol component A and the prepolymer component B are combined in a mass ratio of 1:1 to 2.5; wherein the polyol component A is made of the following raw materials in parts by mass: The chain extender is one or more of a small molecule diol and a small molecule diamine; The cross-linking agent is one or more of low molecular weight polyether polyol, trimethylolpropane, triethanolamine, triisopropanolamine, and glycerol; The stabilizer is a light stabilizer and an antioxidant; The prepolymer B component is made of the following raw materials in parts by mass: 40-60 parts of polyether diol 40-60 parts of isocyanate.

2. The railway rail elastic pad according to claim 1, characterized in that: The polyether diol in the polyol component A is one or more of polytetrahydrofuran diol and tetrahydrofuran-propylene oxide copolyether diol, and has a molecular weight of 1000 to 3000; The polyether polyol in the polyol component A is one or more of polyoxypropylene triol, polyoxyethylene oxypropylene triol, polytetrahydrofuran triol, and tetrahydrofuran-oxypropylene copolyether diol, and has a molecular weight of 2000-6000.

3. The rail elastic pad for railway according to claim 1, characterized in that: The foam stabilizer in the polyol A component is an organosilicon foam stabilizer; The pigment in the polyol component A is any one of a color paste and a powder pigment.

4. The railway rail elastic pad according to any one of claims 1 to 3, characterized in that: The blowing agent in the polyol A component is water.

5. The railway rail elastic pad according to any one of claims 1 to 3, characterized in that: The catalyst in the polyol component A is any one of an amine catalyst and an organic tin catalyst.

6. The railway rail elastic pad according to any one of claims 1 to 3, characterized in that: The polyether diol in the prepolymer component B is one or more of polytetrahydrofuran diol and tetrahydrofuran-propylene oxide copolyether diol, and has a molecular weight of 1000 to 3000; The isocyanate in the prepolymer component B is one or more of toluene diisocyanate, diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate.

7. A method for preparing the railway rail elastic pad according to any one of claims 1 to 6, characterized in that: The steps include: The polyol component A and the prepolymer component B are prepared separately; wherein, The raw materials are taken according to the formula of the polyol component A of the railway rail elastic pad according to any one of claims 1 to 6. The preparation of the polyol component A includes: Add the polyether diol, polyether polyol, chain extender, crosslinker, stabilizer and foam stabilizer into a reaction kettle, stir at 40-90° C., test the moisture content after mixing evenly, then add the pigment, foaming agent and catalyst into the reaction kettle, mix evenly, and seal and store the discharged materials; The formula of the prepolymer component B of the railway rail elastic pad according to any one of claims 1 to 6 is to take various raw materials, and the preparation of the prepolymer component B includes: The polyether polyol and isocyanate are reacted at 70-90° C. for 2 hours, and the NCO content is tested. After the content is qualified, the material is discharged and sealed for storage; After the material temperature is constant at 30-80°C, the polyol component A and the prepolymer component B prepared above are mixed evenly at a mass ratio of 1:1-2.5 and then injected into the elastic pad under the rail mold. The temperature of the elastic pad under the rail mold is 60-120°C. After 8-30 minutes, the mold is removed and placed in a constant temperature room or 100°C for maturation for 12-24 hours to obtain the elastic pad under the rail for railways.