High-speed impact-resistant polyurethane elastomer composite material and preparation method thereof
By using the combination of catechol organic compounds, amine compounds and carbon nanofibers oxidized into quinone in polyurethane elastomers, the high-speed impact resistance of polyurethane elastomer composites is improved, and the high-speed impact of polyurethane elastomers is solved The failure problem under this method achieves higher toughness and impact resistance.
Patent Information
- Application Number
- CN202211042703.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Existing polyurethane elastomers are prone to failure damage such as irreversible deformation, thermal softening, cracks and perforation under high-speed impact, and the interface compatibility between nanofillers and polyurethane elastomers is poor, which limits their high-speed impact resistance.
Using the combination of catechol organic compounds, amine compounds, carbon nanofibers and polyurethane elastomer raw materials oxidized into quinone, nanoparticle materials are generated through stirring reaction, and mixed with polyurethane prepolymers and auxiliary materials to improve interface compatibility. to enhance resistance to high-speed impact.
It significantly improves the high-speed impact resistance of polyurethane elastomer composite materials, enhances toughness and compression strength, reduces preparation costs, and there is no obvious macroscopic damage to the samples after impact.
Smart Images

Figure CN115678256B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of military protection or coating, and in particular to a high-speed impact-resistant polyurethane elastomer composite material and a preparation method thereof. Background Art
[0002] Nowadays, in high-risk competitive sports, special operations and other industries, safe and lightweight high-performance high-speed impact resistant protective materials are particularly important, such as helmets, bulletproof vests, armor coatings, etc. High-performance protective materials need to have excellent strength and stiffness to resist impact damage, avoid serious deformation or penetration of protective materials, and also need ultra-high toughness to absorb impact energy, so as to protect human safety. As a viscoelastic material with high strength, tear resistance, wear resistance, high damping capacity, high chemical resistance and other characteristics, polyurethane elastomer can be prepared into various preparations with adjustable hardness and softness, and has a wide application market in the field of human protection and high-speed impact protection devices. Most commercial polyurethane elastomers are thermosetting resins. Although they have good mechanical properties, they are not effective in resisting high-speed impact. In the process of high-speed impact, it is often accompanied by harsh conditions such as high temperature, high pressure, and high strain rate, which can easily cause irreversible deformation, thermal softening, cracks, and even impact perforation of the elastomer, which also limits the application field of polyurethane elastomers. Therefore, protective materials should have better high-speed impact resistance, higher toughness and strength, and good thermal stability. At present, the common means to improve the mechanical properties of polyurethane elastomers are micro / nano fillers, polymer blending and chemical composition adjustment. Among them, nanofillers are mostly defect-free, easy to prepare, have good practical effects, and are more widely used. However, due to the quantum tunneling effect, charge transfer and mutual coupling of interface atoms, nanofillers have serious agglomeration phenomena. Therefore, they generally have very poor dispersibility and interface compatibility when mixed with polyurethane elastomers. It is difficult to fully demonstrate the advantages of nanofillers as a reinforcing phase, which reduces the protective effect of polyurethane elastomers.
[0003] Therefore, there is an urgent need to improve the interfacial compatibility of nanofillers and polyurethane elastomers to solve the irreversible deformation, thermal softening, cracks and even perforation failure damage caused by high-speed impact of polyurethane composites, thereby improving their high-speed impact resistance. Summary of the invention
[0004] The purpose of the present invention is to overcome the failure damage problems of polyurethane elastomers in the prior art such as irreversible deformation, thermal softening, cracks and even impact perforation when resisting high-speed impact, and to provide a high-speed impact resistant polyurethane elastomer composite material and a preparation method thereof. The composite material has strong high-speed impact resistance, and the preparation cost of the method is low, the preparation method is simple, and the prepared composite material has obvious high-speed impact resistance effect, and can be widely used in industrial production.
[0005] In order to achieve the above-mentioned object, the present invention provides a high-speed impact polyurethane elastomer composite material, the raw material components of which include: a catechol organic compound that can be oxidized to quinone, an amine compound, carbon nanofibers and a polyurethane elastomer raw material, the polyurethane elastomer raw material includes component A and component B, the component A is a polyurethane prepolymer, and the component B includes a polyol and auxiliary materials;
[0006] Relative to 100 parts by mass of the polyurethane elastomer raw material, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
[0007] Preferably, the catechol organic compound that can be oxidized to quinone is at least one selected from catechol, pyrogallol, dopamine, 3,4-dihydroxycinnamic acid, tannic acid, gallic acid and norepinephrine.
[0008] Preferably, the amine compound is selected from at least one of polyethyleneimine, polyamidoamine, polyamidoimide, polyamine, polyallylamine, polyethyleneamine, diethanolamine, gelatin, aminopropyltrisilane and polyetheramine.
[0009] Preferably, the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine.
[0010] Preferably, the polyurethane prepolymer comprises polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4.
[0011] Preferably, the isocyanate is diisocyanate, the polyether diol is polytetramethylene ether diol, and the polyol is polyglycol.
[0012] More preferably, the diisocyanate is at least one selected from 2,4-xylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate.
[0013] Preferably, the polyglycol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol.
[0014] More preferably, the -NCO content in the isocyanate is 5-7% by mass, and the -OH content in the polyglycol is 6-7.5% by mass.
[0015] More preferably, the isocyanate is 2,4-ditoluene isocyanate, and the polyglycol is polycarbonate diol.
[0016] Preferably, the mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains a tetrahydrofuran homopolymer, a chain extender and a catalyst.
[0017] More preferably, relative to 100 parts by mass of the polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass.
[0018] More preferably, the chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
[0019] Further preferably, the mass ratio of the organotin catalyst to the amine catalyst is 1:50-400.
[0020] Further preferably, the aliphatic amine chain extender is N,N'-di-sec-pentylcyclohexanediamine and / or triisopropanolamine, the organotin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine.
[0021] A second aspect of the present invention provides a method for preparing a high-speed impact resistant polyurethane elastomer composite material, comprising the following steps:
[0022] (1) In an alkaline solvent, a catechol organic compound capable of oxidizing to quinone, an amine compound and carbon nanofibers are stirred for reaction I, and then solid-liquid separation is performed to obtain a nanoparticle material;
[0023] (2) mixing the nanoparticle material obtained in step (1) with component B, adding component A to carry out stirring reaction II, exhausting and molding to obtain the high-speed impact resistant polyurethane elastomer composite material;
[0024] The component A is a polyurethane prepolymer, the component B includes a polyol and auxiliary materials, and relative to 100 parts by mass of the component A and the component B, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
[0025] Preferably, the catechol organic compound that can be oxidized to quinone is at least one selected from catechol, pyrogallol, dopamine, 3,4-dihydroxycinnamic acid, tannic acid, gallic acid and norepinephrine.
[0026] Preferably, the amine compound is selected from at least one of polyethyleneimine, polyamidoamine, polyamidoimide, polyamine, polyallylamine, polyethyleneamine, diethanolamine, gelatin, aminopropyltrisilane and polyetheramine.
[0027] Preferably, the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine.
[0028] Preferably, the polyurethane prepolymer comprises polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4.
[0029] Preferably, the isocyanate is diisocyanate, the polyether diol is polytetramethylene ether diol, and the polyol is polyglycol.
[0030] More preferably, the diisocyanate is at least one selected from 2,4-xylene isocyanate, xylylene isocyanate, isophorone diisocyanate and hexamethylene diisocyanate.
[0031] Preferably, the polyglycol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol.
[0032] More preferably, the -NCO content in the isocyanate is 5-7% by mass, and the -OH content in the polyglycol is 6-7.5% by mass.
[0033] More preferably, the isocyanate is 2,4-ditoluene isocyanate, and the polyglycol is polycarbonate diol.
[0034] Preferably, the mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains a tetrahydrofuran homopolymer, a chain extender and a catalyst.
[0035] More preferably, relative to 100 parts by mass of the polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass.
[0036] More preferably, the chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
[0037] Further preferably, the mass ratio of the organotin catalyst to the amine catalyst is 1:50-400.
[0038] Further preferably, the aliphatic amine chain extender is N,N'-di-sec-pentylcyclohexanediamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine.
[0039] Preferably, in step (1), the pH of the alkaline solvent is 8-9, and the stirring reaction conditions I include: the time is 12-48 hours.
[0040] Preferably, in step (2), the mixing is ultrasonic mixing, and the conditions of the ultrasonic mixing include: ultrasonic power of 200-400W, and ultrasonic time of 0.5-2h.
[0041] Preferably, in step (2), the stirring conditions of reaction II include: a stirring rate of 500-4000 rpm and a stirring time of 0.2-0.5 h.
[0042] The third aspect of the present invention provides a high-speed impact resistant polyurethane elastomer composite material prepared by the preparation method described in the second aspect.
[0043] Through the above technical scheme, the present invention can effectively improve the interfacial compatibility of the high-speed impact-resistant polyurethane elastomer composite material through the interaction between the catechol organic compounds that can be oxidized to quinones, amine compounds, carbon nanofibers and polyurethane elastomer raw materials, thereby achieving the effects of strengthening, toughening and high-speed impact resistance.
[0044] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is an infrared spectrum of the nanoparticle material and carbon nanofiber prepared in Example 1, CNFs is carbon nanofiber, CC-PEI@CNFs is nanoparticle material;
[0046] Figure 2 is the ultraviolet absorption spectrum of the nanoparticle material prepared in Example 1, CC-PEI@CNFs is a nanoparticle material;
[0047] Figure 3 It is the full XPS spectrum of the nanoparticle material and carbon nanofiber prepared in Example 1, CNFs is carbon nanofiber, CC-PEI@CNFs is nanoparticle material;
[0048] Figure 4 is the thermogravimetric curve of the nanoparticle material and carbon nanofiber prepared in Example 1, CNFs is carbon nanofiber, CC-PEI@CNFs is the nanoparticle material;
[0049] Figure 5 1 is a SEM image of the nanoparticle material and carbon nanofiber prepared in Example 1, A is the carbon nanofiber, and B is the nanoparticle material;
[0050] Figure 61 is the engineering stress-strain curve obtained from the split-Hopkinson bar experiment of Examples 1-8 and Comparative Example 1, a is Example 1, b is Example 2, c is Example 3, d is Example 4, e is Example 5, f is Example 6, g is Example 7, h is Example 8, and i is Comparative Example 1;
[0051] Figure 7 The pictures are of the samples after impact of the split Hopkinson bar in comparative example 1 and example 1, A is pure polyurethane elastomer, and B is a mixture of modified nanoparticle material and polyurethane elastomer. DETAILED DESCRIPTION
[0052] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0053] As mentioned above, the first aspect of the present invention provides a high-speed impact resistant polyurethane elastomer composite material, the raw material components of the material contain: a catechol organic compound that can be oxidized to quinone, an amine compound, carbon nanofibers and a polyurethane elastomer raw material, the polyurethane elastomer raw material contains an A component and a B component, the A component is a polyurethane prepolymer, and the B component includes a polyol and auxiliary materials;
[0054] Relative to 100 parts by mass of the polyurethane elastomer raw material, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
[0055] The catechol organic compounds, amine compounds, carbon nanofibers, isocyanates, polyols and various auxiliary materials mentioned above in the present invention that can be oxidized to quinones can be obtained commercially or prepared by known methods.
[0056] The inventors of the present invention discovered during the course of their research that by using catechol organic compounds that can be oxidized to quinones, amine compounds, carbon nanofibers and polyurethane elastomer raw materials to prepare a high-speed impact resistant polyurethane elastomer composite material, the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material can be effectively improved through the interaction between the catechol organic compounds, amine compounds, carbon nanofibers and polyurethane elastomer raw materials in the above-mentioned proportions.
[0057] The catechol organic compound that can be oxidized to quinone refers to an organic substance having at least two hydroxyl groups located in a connected position on the benzene ring that can be oxidized to quinone through an oxidation reaction. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the catechol organic compound that can be oxidized to quinone is selected from at least one of catechol, pyrogallol, dopamine, 3,4-dihydroxycinnamic acid, tannic acid, gallic acid and norepinephrine. Preferably, it is selected from at least one of catechol, pyrogallol, dopamine and 3,4-dihydroxycinnamic acid.
[0058] The amine compound refers to a polymer containing an amine group in its structure. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the amine compound is selected from at least one of polyethyleneimine, polyamideamine, polyamideimide, polyamine, polyallylamine, polyethyleneamine, diethanolamine, gelatin, aminopropyltrisilane and polyetheramine. Preferably, it is at least one of polyethyleneimine, polyamideamine, polyamideimide, polyamine, polyallylamine and polyethyleneamine.
[0059] In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, as a relatively preferred embodiment of the present invention, the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine.
[0060] The polyurethane prepolymer can be any polyurethane prepolymer. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the polyurethane prepolymer includes polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4. Further preferably, the mass ratio of the isocyanate to the polyether diol is 2-2.5. From the perspective of further improving the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the isocyanate is a diisocyanate, the polyether diol is polytetrahydrofuran ether diol, and the polyol is a polydiol. Further preferably, the diisocyanate is selected from at least one of 2,4-xylene isocyanate, xylene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; the polydiol is selected from at least one of polycarbonate diol, polybutylene adipate diol, polyε-caprolactone diol and polypropylene glycol. More preferably, the -NCO content in the isocyanate is 5-7% by mass, specifically 5%, 5.5%, 6%, 6.5%, 7%, or any value between the aforementioned values; the -OH content in the polyglycol is 6-7.5% by mass, specifically 6%, 6.5%, 7%, 7.5%, or any value between the aforementioned values. More preferably, the isocyanate is 2,4-xylene isocyanate, and the polyglycol is polycarbonate diol.
[0061] According to the present invention, the auxiliary material can be an auxiliary material commonly used in the preparation process of polyurethane materials, such as a catalyst, a filler, a chain extender, etc.; the mass ratio between component A and component B can also be determined according to the prior art. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains a tetrahydrofuran homopolymer, a chain extender and a catalyst. From the perspective of further improving the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, relative to 100 parts by mass of polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass. Further preferably, the chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
[0062] Preferably, the mass ratio of the organotin catalyst to the amine catalyst is 1:50-400, specifically 1:100, 1:150, 1:200, 1:250, 1:300, 1:350, 1:400, or any value between the aforementioned values. The high-speed impact resistant polyurethane elastomer composite material prepared under this ratio condition has better high-speed impact resistance. The mass ratio of the organotin catalyst to the amine catalyst is preferably 1:200-300.
[0063] From the perspective of further improving the high-speed impact resistance of the high-speed impact-resistant polyurethane elastomer composite material, preferably, the aliphatic amine chain extender is selected from at least one of N,N'-di-secondary pentyl cyclohexane diamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine. More preferably, the aliphatic amine chain extender is N,N'-di-secondary pentyl cyclohexane diamine, the organic tin catalyst is dibutyltin dilaurate, and the amine catalyst is triethylamine.
[0064] As mentioned above, the second aspect of the present invention provides a method for preparing a high-speed impact resistant polyurethane elastomer composite material, comprising the following steps:
[0065] (1) In an alkaline solvent, a catechol organic compound capable of oxidizing to quinone, an amine compound and carbon nanofibers are stirred for reaction I, and then solid-liquid separation is performed to obtain a nanoparticle material;
[0066] (2) mixing the nanoparticle material obtained in step (1) with component B, adding component A to carry out stirring reaction II, exhausting and molding to obtain the high-speed impact resistant polyurethane elastomer composite material;
[0067] The component A is a polyurethane prepolymer, the component B includes a polyol and auxiliary materials, and relative to 100 parts by mass of the component A and the component B, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
[0068] According to the present invention, in step (1), solid-liquid separation can be carried out by any solid-liquid separation method, such as centrifugation, filtration, filter pressing, etc. Preferably, step (1) also includes washing and drying the solid obtained by solid-liquid separation, the washing agent used for washing is water, and the number of washing times is 2-5 times. Drying can be air drying, oven drying, etc.
[0069] In step (2), exhaust can be performed by any exhaust method, such as vibration exhaust, vacuum exhaust or other exhaust methods. Molding can be performed by mold molding. Preferably, the molding conditions include: the time is 5-30 minutes.
[0070] The inventors of the present invention found in the research process that the high-speed impact resistant polyurethane elastomer composite material prepared by the above preparation method has better compression strength, toughness and high-speed impact resistance, and the preparation method is relatively simple.
[0071] The catechol organic compound that can be oxidized to quinone refers to an organic substance having at least two hydroxyl groups located in a connected position on the benzene ring that can be oxidized to quinone through an oxidation reaction. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the catechol organic compound that can be oxidized to quinone is selected from at least one of catechol, pyrogallol, dopamine, 3,4-dihydroxycinnamic acid, tannic acid, gallic acid and norepinephrine. Preferably, it is selected from at least one of catechol, pyrogallol, dopamine and 3,4-dihydroxycinnamic acid.
[0072] The amine compound refers to a compound containing an amine group in its structure. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the amine compound is selected from at least one of polyethyleneimine, polyamideamine, polyamideimide, polyamine, polyallylamine, polyethyleneamine, diethanolamine, gelatin, aminopropyltrisilane and polyetheramine. Preferably, it is at least one of polyethyleneimine, polyamideamine, polyamideimide, polyamine, polyallylamine and polyethyleneamine.
[0073] In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, as a relatively preferred embodiment of the present invention, the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine.
[0074] The polyurethane prepolymer can be any polyurethane prepolymer. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the polyurethane prepolymer includes polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4, specifically 1:0.4, 1:0.8, 1:1.2, 1:1.6, 1:2, 1:2.4, 1:2.8, 1:3.2, 1:3.6, 1:4, or any value in the range formed by any two of these ratios, more preferably 1:1.6-2.8. Considering further improving the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the isocyanate is diisocyanate, the polyether diol is polytetrahydrofuran ether diol, and the polyol is polydiol. Further preferably, the diisocyanate is selected from at least one of 2,4-xylene isocyanate, xylene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; the polyglycol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol. More preferably, the -NCO content in the isocyanate is 5-7% by mass, specifically 5% by mass, 5.5% by mass, 6% by mass, 6.5% by mass, 7% by mass, or any value between the aforementioned values; the -OH content in the polyglycol is 6-7.5% by mass, specifically 6% by mass, 6.5% by mass, 7% by mass, 7.5% by mass, or any value between the aforementioned values. Further preferably, the isocyanate is 2,4-xylene isocyanate, and the polyglycol is polycarbonate diol.
[0075] According to the present invention, the auxiliary material can be an auxiliary material commonly used in the preparation process of polyurethane materials, such as a catalyst, a filler, a chain extender, etc.; the mass ratio between component A and component B can also be determined according to the prior art. In order to further improve the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, preferably, the mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains a tetrahydrofuran homopolymer, a chain extender and a catalyst. From the perspective of further improving the high-speed impact resistance of the high-speed impact resistant polyurethane elastomer composite material, relative to 100 parts by mass of polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass. Further preferably, the chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
[0076] Preferably, the mass ratio of the organotin catalyst to the amine catalyst is 1:50-400, specifically 1:50, 1:100, 1:150, 1:200, 1:250, 1:300, 1:350, 1:400, or any value between the aforementioned values. The high-speed impact resistant polyurethane elastomer composite material prepared under this ratio condition has better high-speed impact resistance. The mass ratio of the organotin catalyst to the amine catalyst is preferably 1:200-300.
[0077] In order to further improve the mechanical properties of the polyurethane elastomer composite material resistant to high-speed impact, preferably, the aliphatic amine chain extender is N, N'-di-secondary pentyl cyclohexane diamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N, N-dimethylcyclohexylamine, triethanolamine and triethylamine. More preferably, the aliphatic amine chain extender is N, N'-di-secondary pentyl cyclohexane diamine, the organic tin catalyst is dibutyltin dilaurate, and the amine catalyst is triethylamine.
[0078] The alkaline solvent can be any solvent that can provide alkaline conditions, preferably a buffer solution with a pH higher than 7, and the buffer solution can be a phosphate buffer, a Tri-HCl buffer or a carbonate buffer, etc. Preferably, it is a Tri-HCl buffer. Preferably, in step (1), the pH of the alkaline solvent is 8-9, and the conditions of the stirring reaction I include: the time is 12-48h. The high-speed impact resistant polyurethane elastomer composite material prepared under the above reaction conditions has better high-speed impact resistance.
[0079] The mixing may be ultrasonic mixing, stirring mixing or oscillating mixing. In order to further improve the mixing effect, preferably, in step (2), the mixing is ultrasonic mixing, and the conditions of the ultrasonic mixing include: ultrasonic power of 200-400W, and ultrasonic time of 0.5-2h.
[0080] Preferably, in step (2), the stirring reaction II comprises: a stirring rate of 500-4000 rpm and a stirring time of 0.2-0.5 h. The high-speed impact resistant polyurethane elastomer composite material prepared under such conditions has higher high-speed impact resistance.
[0081] As mentioned above, the third aspect of the present invention provides a high-speed impact resistant polyurethane elastomer composite material prepared by the preparation method described in the second aspect. The high-speed impact resistant polyurethane elastomer composite material has better compression strength, toughness and high-speed impact resistance.
[0082] According to a particularly preferred embodiment of the present invention, a method for preparing a high-speed impact-resistant polyurethane elastomer composite material is provided, comprising the following steps:
[0083] (1) In a Tri-HCl buffer solution with a pH of 8-9, a catechol organic compound capable of being oxidized to quinone, an amine compound and carbon nanofibers are mixed and stirred for 12-48 hours, and then filtered and washed with water for 2-5 times to obtain a nanoparticle material;
[0084] (2) ultrasonically mixing the nanoparticle material obtained in step (1) and component B at a power of 50-400 W for 0.5-2 h, adding component A and mixing at a speed of 500-4000 rpm for 0.2-0.5 h, exhausting, and molding in a mold to obtain the high-speed impact resistant polyurethane elastomer composite material;
[0085] Relative to 100 parts by mass of the component A and the component B, the catechol organic compound capable of being oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass; the mass ratio of the component A to the component B is 2-4:1; the catechol organic compound capable of being oxidized to quinone is selected from catechol, pyrogallol, dopamine, 3,4-dihydroxycinnamic acid, mono At least one of tannic acid, gallic acid and norepinephrine, the amine compound is selected from at least one of polyethyleneimine, polyamide amine, polyamide imine, polyamine, polyallylamine, polyethyleneamine, diethanolamine, gelatin, aminopropyltrisilane and polyetheramine, the A component is isocyanate and polytetramethylene ether diol, the mass ratio of the isocyanate to the polytetramethylene ether diol is 1:0.4-4, the isocyanate is selected from 2,4-xylene isocyanate, xylene diisocyanate , at least one of isophorone diisocyanate and hexamethylene diisocyanate, the B component comprises a polyol and an auxiliary material, the polyol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol, the auxiliary material contains a tetrahydrofuran homopolymer, a chain extender and a catalyst, relative to 100 parts by mass of the polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass The chain extender is an aliphatic amine chain extender, the catalyst is an organic tin catalyst and an amine catalyst, the mass ratio of the organic tin catalyst to the amine catalyst is 1:50-400, the aliphatic amine chain extender is selected from at least one of N,N'-di-sec-pentylcyclohexanediamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine.
[0086] The inventors of the present invention found in the research process that the composite material prepared by the above method has excellent compressive strength, toughness and impact resistance, and the compression rebound rate is as high as 91.9%. -1 ) has extremely high absorption energy under impact, up to 92.77J / cm 3 , than pure polyurethane elastomer (43.71J / cm 3 ) increased by 112.24%, and there was no obvious macroscopic damage to the sample after impact.
[0087] The present invention will be described in detail below through examples.
[0088] In the following embodiments, the static compression test was conducted according to the method provided in ISO 7743-2008 (E), the instrument used for the test was an electronic universal testing machine (China Hualong, WDW-100C), the sample size was Φ20*4mm, and the compression rate was 87.5%; the dynamic impact test was conducted by a split Hopkinson bar (National University of Defense Technology), which was an aluminum alloy bar with a diameter of 20mm, grade 7A04, Poisson's ratio of 0.33, and a density of 2.8g / cm 3 , where the length of the impact rod is 48.0 cm, the length of the incident rod is 249.5 cm, the length of the transmission rod is 149.5 cm, and the length of the absorption rod is 28.5 cm. During the test, the air pressure was set to 0.2 MPa, and a similar strain rate of about 9000 s was obtained. -1 The sample size is Φ10*2mm; the scanning electron microscope was purchased from Zeiss Company, and the instrument model is Sigma200; the thermogravimetric analyzer was purchased from TA Company in the United States, and the instrument model is TQAQ50; the X-ray photoelectron microscope was purchased from Thermo Fisher Scientific, and the instrument model is K-Alpha; the UV-visible photometer was purchased from Aoyi Instrument (Shanghai) Company, and the instrument model is UV-1800PC; the Fourier transform infrared spectrometer was purchased from Thermo Fisher Scientific, and the instrument model is NICOLEF6700.
[0089] Based on the dynamic impact test, the formula Calculation of engineering stress σ s (t), using the formula Calculation of engineering strain ε s (t), using the formula Calculate strain rate
[0090] Among them, ε r (t) is the input rod strain signal, ε t (t) is the output rod strain signal, A s0is the cross-sectional area of the sample, A0 is the cross-sectional area of the rod, L s0 is the thickness of the sample, C0 is the wave velocity of the rod, and E0 is the Young's modulus of the rod.
[0091] Polyethyleneimine (purity greater than 99.5%, molecular weight 600, Aladdin), catechol and pyrogallol (purity greater than 95.0%, Aladdin), carbon nanofiber (purity greater than 95.0%, Nanjing Xianfeng Nanotechnology Co., Ltd.), dibutyltin dilaurate (95%, Maclean), 3,4-dihydroxycinnamic acid (98%, J&K), polyvinylamine (99%, molecular weight 1800, Maclean), and other chemicals such as polycarbonate diol, tetrahydrofuran homopolymer, N,N'-di-sec-pentylcyclohexanediamine, hexamethylene diisocyanate, 2,4-xylene isocyanate, etc. are all industrially pure and provided by Qingdao Green World Technology Co., Ltd.
[0092] Example 1
[0093] (1) In 150 mL of Tri-HCl buffer (pH 8.5), 0.15 g of catechol, 0.3 g of polyethyleneimine and 1 g of carbon nanofiber were mixed and stirred for 24 h, then filtered and washed with water three times to obtain a nanoparticle material;
[0094] (2) The nanoparticle material and 15.34 g of polycarbonate diol (-OH content is 6.0 mass%), 7.67 g of tetrahydrofuran homopolymer, 0.77 g of N,N'-di-sec-pentylcyclohexanediamine, 0.01 g of dibutyltin dilaurate, and 1.22 g of triethylamine are ultrasonically mixed at a power of 300 W for 1 hour, 25 g of 2,4-xylene isocyanate (-NCO content is 5.0 mass%) and 50 g of polytetrahydrofuran ether diol are added and stirred for 0.3 hour, the mixture is vented, and the high-speed impact-resistant polyurethane elastomer composite material is obtained after molding in a mold.
[0095] The nanoparticle material and carbon nanofiber obtained in step (1) were characterized by Fourier transform infrared spectroscopy, XPS, thermogravimetric analysis and SEM to obtain Figure 1 , Figure 3 ,Table 1, Figure 4 and Figure 5 ; UV characterization of nanoparticle materials was performed to obtain Figure 2 ; It shows that catechol and polyethyleneimine react and deposit on carbon nanofibers.
[0096] Table 1
[0097]
[0098] Among them, CNFs is carbon nanofiber, and CC-PEI@CNFs is nanoparticle material.
[0099] The nanoparticle material and carbon nanofiber obtained in step (1) were subjected to thermogravimetric analysis. Figure 4 At 30-120℃, the nanoparticle material loses nearly 5% of its weight, mainly due to the loss of adsorbed water; at 120-580℃, the weight loss rate is about 16%, which is because the CC-PEI deposited on the surface of the carbon nanofiber decomposes. As the temperature rises from 580-850℃, the CO bonds in the carbon nanofiber decompose by about 5%. Thermogravimetric experiments show that the co-deposition amount of catechol and polyethyleneimine reactants on the surface of carbon nanofibers is about 16%.
[0100] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression rebound rate are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 As shown in the figure, the actual image after the impact is as follows Figure 7 As shown in B.
[0101] Example 2
[0102] (1) In 150 mL of Tri-HCl buffer (pH 8), 0.1 g of catechol, 0.05 g of polyethyleneimine and 1.8 g of carbon nanofibers were mixed and stirred for 24 h, then filtered, washed with water three times, and dried to obtain a nanoparticle material;
[0103] (2) The nanoparticle material and 22.3 g of polycarbonate diol (-OH content is 6.0 mass%), 6.69 g of tetrahydrofuran homopolymer, 1.78 g of N,N'-di-sec-pentylcyclohexanediamine, 0.01 g of dibutyltin dilaurate, and 2.22 g of triethylamine are ultrasonically mixed at a power of 200 W for 2 h, 19.14 g of 2,4-ditoluene isocyanate (-NCO content is 6.5 mass%) and 47.86 g of polytetrahydrofuran ether diol are added and stirred for 0.5 h, the mixture is vented, and the high-speed impact-resistant polyurethane elastomer composite material is obtained after molding in a mold.
[0104] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0105] Example 3
[0106] (1) In 150 mL of Tri-HCl buffer at pH 9, 0.5 g of catechol, 0.25 g of polyethyleneimine and 0.2 g of carbon nanofibers were mixed and stirred for 24 h, then filtered and washed with water three times to obtain a nanoparticle material;
[0107] (2) The nanoparticle material and 11.3 g of polycarbonate diol (-OH content is 7.5 mass%), 7.81 g of tetrahydrofuran homopolymer, 0.24 g of N,N'-di-sec-pentylcyclohexanediamine, 0.01 g of dibutyltin dilaurate, and 0.55 g of triethylamine are ultrasonically mixed at a power of 400 W for 0.5 h, 25 g of 2,4-ditoluene isocyanate (-NCO content is 7.0 mass%) and 55 g of polytetrahydrofuran ether diol are added and stirred for 0.2 h, the mixture is vented, and the high-speed impact-resistant polyurethane elastomer composite material is obtained after molding in a mold.
[0108] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0109] Example 4
[0110] A high-speed impact resistant polyurethane elastomer composite material was prepared according to the method of Example 3, except that 0.4 g of pyrogallol and 0.1 g of 3,4-dihydroxycinnamic acid were used instead of 0.5 g of catechol.
[0111] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0112] Example 5
[0113] A high-speed impact resistant polyurethane elastomer composite material was prepared according to the method of Example 3, except that polyvinylamine was used instead of polyethyleneimine.
[0114] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0115] Example 6
[0116] A high-speed impact resistant polyurethane elastomer composite material was prepared according to the method of Example 3, except that hexamethylene diisocyanate (-NCO content of 10.5 mass %) was used instead of 2,4-ditoluene isocyanate.
[0117] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0118] Example 7
[0119] A high-speed impact resistant polyurethane elastomer composite material was prepared according to the method of Example 3, except that tetrahydrofuran homopolymer was not added.
[0120] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0121] Example 8
[0122] A high-speed impact resistant polyurethane elastomer composite material was prepared according to the method of Example 3, except that the added amount of dibutyltin dilaurate was 0.02 g and the added amount of triethylamine was 0.54 g.
[0123] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test and a separated Hopkinson bar test, and the obtained compression modulus and compression resilience are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 shown.
[0124] Comparative Example 1
[0125] 0.2 g of carbon nanofibers, 11.3 g of polycarbonate diol (-OH content of 7.5 mass%), 7.81 g of tetrahydrofuran homopolymer, 0.24 g of N,N'-di-sec-pentylcyclohexanediamine, 0.01 g of dibutyltin dilaurate, and 0.55 g of triethylamine were ultrasonically mixed at a power of 300 W for 0.5 h, 25 g of 2,4-xylene isocyanate (-NCO content of 7 mass%) and 55 g of polytetrahydrofuran ether diol were added and stirred for 0.2 h, the mixture was vented, and the high-speed impact-resistant polyurethane elastomer composite material was obtained after molding in a mold.
[0126] The high-speed impact resistant polyurethane elastomer composite material was subjected to a static compression test (compression rate of 87.5%) and a separated Hopkinson bar test, and the obtained compression modulus and compression rebound rate are shown in Table 2, the obtained high-speed impact resistant absorption energy is shown in Table 3, and the obtained Hopkinson bar engineering stress-strain curve is shown in Figure 6 As shown in the figure, the actual image after the impact is as follows Figure 7 As shown in A.
[0127] Table 2
[0128] serial number Compression strength(MPa) Compression rebound rate (%) Example 1 42.31 90.0% Example 2 43.30 91.9% Example 3 42.26 90.5% Example 4 34.18 80.0% Example 5 35.03 77.5% Example 6 35.53 81.3% Example 7 32.08 78.1% Example 8 36.86 78.8% Comparative Example 1 17.82 35.2%
[0129] Table 3
[0130]
[0131]
[0132] It can be seen from the results in Table 2 and Table 3 that the compression strength, compression rebound rate and impact absorption energy in Examples 1-8 of the present invention are significantly better than those in Comparative Example 1, indicating that the high-speed impact resistant polyurethane elastomer composite material of the present invention has better strength, toughness and high-speed impact resistance.
[0133] from Figure 6 It can be concluded that the impact strength of the samples in Examples 1-8 is much higher than that in Comparative Example 1. The integral area of the stress-strain curve is the impact absorption energy, which represents the ability of the sample to absorb impact energy, corresponding to the data in Table 3. It can be found that Examples 1-8 have higher impact strength and good absorption energy. Among them, the impact resistance of the sample in Example 1 is the most excellent: the impact strength and absorption energy are well balanced. Compared with the sample in Comparative Example 1, the maximum impact strength is increased by 196.53%, and the absorption energy is increased by 112.24%.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A high-speed impact resistant polyurethane elastomer composite material, characterized in that: The raw material components of the material include: a catechol organic compound that can be oxidized to quinone, an amine compound, carbon nanofibers and a polyurethane elastomer raw material, wherein the polyurethane elastomer raw material includes a component A and a component B, wherein the component A is a polyurethane prepolymer, and the component B contains a polyol and auxiliary materials, wherein the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine; With respect to 100 parts by mass of the polyurethane elastomer raw material, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
2. The high-speed impact resistant polyurethane elastomer composite material according to claim 1, characterized in that: The polyurethane prepolymer comprises polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4.
3. The high-speed impact resistant polyurethane elastomer composite material according to claim 2, characterized in that: The isocyanate is diisocyanate, the polyether diol is polytetramethylene ether diol, and the polyol is polyglycol.
4. The high-speed impact resistant polyurethane elastomer composite material according to claim 3, characterized in that: The diisocyanate is selected from at least one of 2,4-xylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; The polyglycol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol.
5. The high-speed impact resistant polyurethane elastomer composite material according to claim 4, characterized in that: The isocyanate is 2,4-ditoluene isocyanate, and the polyglycol is polycarbonate diol.
6. The high-speed impact resistant polyurethane elastomer composite material according to claim 1, characterized in that: The mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains tetrahydrofuran homopolymer, a chain extender and a catalyst.
7. The high-speed impact resistant polyurethane elastomer composite material according to claim 6, characterized in that: Relative to 100 parts by mass of the polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass.
8. The high-speed impact resistant polyurethane elastomer composite material according to claim 7, characterized in that: The chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
9. The high-speed impact resistant polyurethane elastomer composite material according to claim 8, characterized in that: The mass ratio of the organic tin catalyst to the amine catalyst is 1:50-400.
10. The high-speed impact resistant polyurethane elastomer composite material according to claim 9, characterized in that: The aliphatic amine chain extender is N,N'-di-sec-pentylcyclohexanediamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine.
11. A method for preparing a high-speed impact resistant polyurethane elastomer composite material, characterized in that: The steps include: (1) In an alkaline solvent, a catechol organic compound capable of oxidizing to quinone, an amine compound and carbon nanofibers are stirred for reaction I, and then solid-liquid separation is performed to obtain a nanoparticle material; (2) mixing the nanoparticle material obtained in step (1) with component B, adding component A to carry out stirring reaction II, exhausting and molding to obtain the high-speed impact resistant polyurethane elastomer composite material; The component A is a polyurethane prepolymer, the component B contains polyol and auxiliary materials, the catechol organic compound that can be oxidized to quinone is catechol, and the amine compound is polyethyleneimine. Relative to 100 parts by mass of the component A and the component B, the catechol organic compound that can be oxidized to quinone is 0.1-0.5 parts by mass, the amine compound is 0.05-0.25 parts by mass, and the carbon nanofiber is 0.2-2.5 parts by mass.
12. The preparation method according to claim 11, characterized in that: The polyurethane prepolymer comprises polyether diol and isocyanate, and the mass ratio of the isocyanate to the polyether diol is 1:0.4-4.
13. The preparation method according to claim 12, characterized in that: The isocyanate is diisocyanate, the polyether diol is polytetramethylene ether diol, and the polyol is polyglycol.
14. The preparation method according to claim 13, characterized in that: The diisocyanate is selected from at least one of 2,4-xylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; The polyglycol is selected from at least one of polycarbonate diol, polybutylene adipate diol, poly-ε-caprolactone diol and polypropylene glycol.
15. The preparation method according to claim 14, characterized in that: The isocyanate is 2,4-ditoluene isocyanate, and the polyglycol is polycarbonate diol.
16. The preparation method according to claim 11, characterized in that: The mass ratio of the component A to the component B is 2-4:1, and the auxiliary material contains tetrahydrofuran homopolymer, a chain extender and a catalyst.
17. The preparation method according to claim 16, characterized in that: Relative to 100 parts by mass of the polyol, the tetrahydrofuran homopolymer is 30-70 parts by mass, the chain extender is 2-8 parts by mass, and the catalyst is 5-10 parts by mass.
18. The preparation method according to claim 17, characterized in that: The chain extender is an aliphatic amine chain extender, and the catalyst is an organic tin catalyst and an amine catalyst.
19. The preparation method according to claim 18, characterized in that: The mass ratio of the organic tin catalyst to the amine catalyst is 1:50-400.
20. The preparation method according to claim 19, characterized in that: The aliphatic amine chain extender is N,N'-di-sec-pentylcyclohexanediamine and / or triisopropanolamine, the organic tin catalyst is dibutyltin dilaurate and / or stannous octoate, and the amine catalyst is selected from at least one of N,N-dimethylcyclohexylamine, triethanolamine and triethylamine.
21. The preparation method according to claim 11, characterized in that: In step (1), the pH of the alkaline solvent is 8-9, and the stirring reaction conditions I include: the time is 12-48h; In step (2), the mixing is ultrasonic mixing, and the conditions of the ultrasonic mixing include: ultrasonic power of 200-400W, ultrasonic time of 0.5-2h; The conditions of the stirring reaction II include: a stirring rate of 500-4000 rpm and a stirring time of 0.2-0.5 h.
22. The high-speed impact resistant polyurethane elastomer composite material prepared by the preparation method according to any one of claims 11 to 21.