A phosphosilicate anti-rust pigment and its preparation method and application
By simplifying the preparation process of phosphosilicate anti-rust pigment, combined with the combination of phosphoric acid, silicon source, aluminum source and calcium source, the problem of poor anti-rust effect in water-based coatings is solved, and higher anti-rust performance and stability are achieved reduces production costs.
Patent Information
- Application Number
- CN202211375457.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-04
AI Technical Summary
The existing aluminum-calcium phosphosilicate anti-rust pigments have poor anti-rust effect in water-based coatings, poor stability, and complex preparation process, making it difficult to meet the cost-effectiveness needs of water-based acrylic coatings.
The phosphosilicate anti-rust pigment is prepared by mixing evenly, adding phosphoric acid solution dropwise, adjusting pH value and adding modifiers, simplifying the process flow and improving anti-rust performance and stability.
It significantly improves the anti-rust performance, thermal stability and anti-aging properties in water-based coatings, shortens production time, reduces costs, and obtains more stable product quality.
Smart Images

Figure BDA0003926496130000081 
Figure BDA0003926496130000091 
Figure HDA0003926496140000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-rust pigments, and particularly relates to a phosphosilicate anti-rust pigment and a preparation method and application thereof. Background Art
[0002] Since the 1970s, in view of the continuous strengthening of environmental awareness and industrial hygiene laws and regulations, companies in various countries have been competing to develop non-toxic, environmentally friendly and efficient anti-rust pigments. In addition, traditional solvent-based coatings contain volatile organic compounds (VOCs), which will evaporate during the film-forming process. Volatile organic compounds will also cause secondary pollution to the atmospheric environment. Long-term exposure of humans and animals to high-VOC environments will greatly increase the possibility of cancer complications. Therefore, the traditional coating industry is in urgent need of upgrading and transformation, and water-based coatings have low or even zero VOC emissions. While improving the production environment, it also reduces the cost of solvents and reduces production costs, making water-based coatings more competitive. Water-based coatings are safe, non-toxic, odorless, non-flammable, and easy to clean. In addition, water-based coatings are cheaper and easier to obtain than solvent-based coatings. With the improvement of national environmental awareness and the introduction of national environmental protection policies, it is a general trend for water-based coatings to replace solvent-based coatings. Its domestic market share has increased rapidly, and its output has increased rapidly. The anti-rust pigments corresponding to water-based anti-corrosion coatings are also facing huge market demand.
[0003] Traditional lead and chromate pigments have very outstanding anti-rust properties, but heavy metals such as lead and chromium in the pigments are toxic. In today's world where environmental protection and people's increasing attention to healthy living are concerned, such anti-rust pigments are gradually banned. Phosphate anti-rust pigments have become effective products that can replace red lead and zinc chrome yellow due to their low toxicity, good compatibility with different resins, superior performance when used in rusty primers, and stable and non-toxic pyrophosphates generated at high temperatures. Publication No. CN 104212222A Chinese patent discloses a calcium aluminum phosphosilicate composite anti-rust pigment, which mixes and compounds calcium aluminum phosphate, calcium silicate and aluminum silicate for use in medium-oil oily alkyd paints. Publication No. CN110343412A Chinese patent discloses a calcium aluminum polyphosphate anti-rust pigment, which is synthesized in steps, mixed and compounded, and finally modified to obtain the final product. The preparation process is complicated, and the product obtained after modification with silane is used in solvent-based coatings. The literature (Wang Junhong, Liao Huan, et al., Preparation and Performance Determination of Calcium Aluminum Phosphosilicate Antirust Pigments, Chemical Technology and Development, 2020, 49 (8), 3-5) discloses calcium aluminum phosphosilicate antirust pigments, which are coated and deposited on the surface of calcium aluminum phosphate using nano-aluminum silicate and nano-calcium silicate for use in water-based alkyd resins. In summary, the current preparation process of calcium aluminum phosphosilicate antirust pigments is complicated, and they are mainly used in oily (solvent-based) coatings. The application of water-based coatings is mainly applied to water-based epoxy resins or water-based alkyd resins. In water-based systems, especially water-based acrylic coatings that pursue cost-effectiveness, there are still problems such as the anti-rust effect does not meet the requirements, poor stability in use, insufficient storage time, and high prices of imported products. Summary of the invention
[0004] The present invention aims at providing a phosphosilicate anti-rust pigment and a preparation method thereof. The phosphosilicate anti-rust pigment is applied to water-based paint and has excellent anti-rust performance, stability and other characteristics.
[0005] To achieve the above object, the present invention provides a phosphosilicate anti-rust pigment, comprising the following raw materials in parts by weight: 60 to 100 parts of phosphoric acid, 20 to 40 parts of silicon source, 10 to 70 parts of aluminum source, 10 to 70 parts of calcium source, 1 to 10 parts of pH adjuster, and 1 to 10 parts of modifier.
[0006] Preferably, in the above-mentioned phosphosilicate anti-rust pigment, the silicon source is a mixture of one or more of silicon dioxide, silica sol, potassium silicate, sodium silicate, calcium silicate, magnesium silicate, lithium silicate, strontium silicate and ammonium silicate.
[0007] Preferably, in the above-mentioned phosphosilicate anti-rust pigment, the aluminum source is one or a mixture of two or more of aluminum oxide, aluminum hydroxide, aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum carbonate, aluminum citrate, sodium aluminate, pseudo-boehmite, isopropoxide aluminum, and aluminum acetate.
[0008] Preferably, in the above-mentioned phosphosilicate anti-rust pigment, the calcium source is one or a mixture of two or more of calcium oxide, calcium hydroxide, calcium carbonate, calcium oleate, calcium nitrate, calcium sulfate, calcium chloride, calcium oxalate, calcium citrate and calcium tartrate.
[0009] Preferably, in the above-mentioned phosphosilicate anti-rust pigment, the pH adjuster is one or a mixture of two or more of acetic acid, oxalic acid, citric acid, tartaric acid, malic acid, succinic acid, lactic acid, and the modifier is vinyl silane, aminosilane or methacryloxysilane.
[0010] The present invention also provides a method for preparing the above-mentioned phosphosilicate anti-rust pigment, comprising the following steps:
[0011] (1) weighing a silicon source, an aluminum source and a calcium source, adding deionized water in an amount of 1 to 2 times the total mass of the silicon source, the aluminum source and the calcium source, stirring and mixing at a certain speed to make a uniformly dispersed slurry;
[0012] (2) Weigh phosphoric acid to prepare an aqueous solution with a mass percentage concentration of 25 to 50%, and slowly dropwise add the phosphoric acid solution to the slurry at a temperature of 40 to 95° C. under stirring; after the phosphoric acid solution is added, adjust the pH of the slurry to 4 to 5 with a pH adjuster, and continue stirring the reaction under constant temperature conditions;
[0013] (3) adjusting the slurry temperature of step (2) to 40-70° C., adding a modifier, and continuing to stir the reaction under constant temperature conditions;
[0014] (4) filtering, washing and drying the slurry obtained in step (3) to obtain a modified calcium aluminum phosphosilicate anti-rust pigment.
[0015] Preferably, in the preparation method of the above-mentioned phosphosilicate anti-rust pigment, in the step (1), the rotation speed is 120 to 250 r / min, and the stirring time is 0.5 to 1 h.
[0016] Preferably, in the preparation method of the above-mentioned phosphosilicate anti-rust pigment, in the step (2), the stirring speed is 120 to 250 r / min, and the stirring reaction time is continued to be 0.5 to 1.5 h.
[0017] Preferably, in the preparation method of the above-mentioned phosphosilicate anti-rust pigment, in the step (3), the stirring reaction time is 0.5 to 2 hours; and in the step (4), the drying temperature is 55 to 120°C.
[0018] Application of the above-mentioned phosphosilicate anti-rust pigment in water-based coatings.
[0019] Preferably, in the above application, the water-based paint is a water-based epoxy resin paint or a water-based acrylic paint.
[0020] Compared with the existing technology, the present invention has the following beneficial effects:
[0021] 1. The phosphosilicate anti-rust pigment of the present invention simultaneously introduces silicon source, aluminum source and calcium source, thereby improving the disadvantage of poor initial anti-rust performance of the previous anti-rust pigment, so that the initial anti-rust performance of the product in water-based coatings is significantly improved.
[0022] 2. The phosphosilicate anti-rust pigment of the present invention is applied to water-based coatings, especially water-based acrylic coatings and water-based epoxy resins. Compared with the existing zinc phosphate and modified aluminum tripolyphosphate anti-rust pigments, the anti-rust performance, thermal stability, weather resistance and aging resistance of the water-based coatings are improved.
[0023] 3. The preparation method of the phosphosilicate anti-rust pigment of the present invention completes the synthesis in one step, which greatly reduces the process and operation steps, shortens the production time, and reduces the production cost compared with the traditional step-by-step reaction process or the complex synthesis method; the average particle size D50 of the prepared phosphosilicate anti-rust pigment particles is about 5 μm, the particle size distribution range is narrow, and the product quality is stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the particle size distribution diagram of the modified calcium aluminum phosphosilicate prepared in Example 1 of the present invention.
[0025] Figure 2 This is the particle size distribution diagram of the modified calcium aluminum phosphosilicate prepared in Example 2 of the present invention.
[0026] Figure 3 This is a 96h salt spray resistance test result diagram of the water-based acrylic anti-corrosion coating in Application Example 1 of the present invention, wherein A is the modified calcium aluminum phosphosilicate anti-rust pigment of Example 1, B is the addition of zinc phosphate, C is modified aluminum tripolyphosphate, and D is the calcium aluminum phosphosilicate anti-rust pigment of Comparative Example 1.
[0027] Figure 4 This is a graph showing the salt spray resistance 300h test result of the waterborne epoxy resin coating in Application Example 2 of the present invention, wherein A is the modified calcium aluminum phosphosilicate antirust pigment of Example 1, B is the addition of zinc phosphate, and C is modified aluminum tripolyphosphate. DETAILED DESCRIPTION
[0028] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0029] Example 1
[0030] 1.5kg silica sol (silicon dioxide content 30wt.%), 2.0kg alumina, 2.0kg calcium carbonate and 5.5kg water were added into the reactor, stirred at a speed of 200r / min, stirred for 0.5h, and a slurry was obtained; the slurry was heated to 50°C and stirred continuously; 5.2kg industrial phosphoric acid was prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5h, and the stirring reaction was continued at a constant temperature for 1h after the dropping was completed; 0.25kg citric acid was added to adjust the pH value to 4.5, and the stirring reaction was continued at a constant temperature for 1h; then, 0.5kg γ-aminopropyltriethoxysilane was slowly added at 50°C for modification, and the stirring reaction was continued for 1h after the addition was completed to make the reaction more fully proceed; filtered, washed, and dried at 105°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0031] The particle size distribution of the modified calcium aluminum phosphosilicate antirust pigment prepared in this example is shown in Figure 1 As can be seen from the figure, the average particle size (D50) of the modified calcium aluminum phosphosilicate anti-rust pigment particles of this embodiment is 4.821 μm, the particles are fine, and the particle size distribution range is narrow.
[0032] Example 2
[0033] 1.1 kg sodium silicate, 1.0 kg aluminum sulfate, 1.6 kg calcium hydroxide and 4.7 kg water were added into the reactor, the stirring speed was 200 r / min, and the stirring was continued for 0.5 h to obtain a slurry; the slurry was heated to 45°C and stirred continuously; 3.2 kg industrial phosphoric acid was prepared into a 30% aqueous solution, and then added dropwise into the slurry for 1 h, and the stirring reaction was continued for 1 h under constant temperature after the addition was completed; 0.2 kg lactic acid was added to adjust the pH value to 4.9, and the stirring was continued for 2 h; then, 0.35 kg γ-methacryloxypropyltrimethoxysilane was slowly added at a temperature of 45°C for modification, and the stirring was continued for 1 h after the addition was completed to make the reaction more fully proceed; finally, the mixture was filtered, washed, and dried at 60°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0034] The particle size distribution of the modified calcium aluminum phosphosilicate antirust pigment prepared in this example is shown in Figure 2 As can be seen from the figure, the average particle size (D50) of the modified calcium aluminum phosphosilicate anti-rust pigment particles of this embodiment is 4.814 μm, the particles are fine, D90 is 10.755 μm, and the particle size distribution range is narrow.
[0035] Example 3
[0036] 2.0kg silica sol, 1.2kg aluminum hydroxide, 1.3kg calcium oxide and 5.0kg water were added into the reactor, the stirring speed was 200r / min, and the mixture was stirred for 0.5h to obtain a slurry; the slurry was heated to 90°C and stirred continuously, 5.0kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5h, and the reaction was continued under constant temperature stirring for 1h after the addition was completed; 0.12kg oxalic acid was added to adjust the pH value to 4.2, and the reaction was continued under stirring for 0.5h; then, the temperature was lowered to 70°C, and 0.24kg vinyl tris-(2-methoxyethoxy)-silane was slowly added for modification, and the reaction was continued for 1h after the addition was completed to make the reaction more fully proceed; finally, the mixture was filtered and washed, and dried at 120°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0037] Example 4
[0038] 1.0kg ammonium silicate, 0.5kg aluminum nitrate, 2.0kg calcium oleate and 4.2kg water were added into the reactor, the stirring speed was 200r / min, and the stirring was continued for 0.5h to obtain a slurry; the slurry was heated to 60°C and stirred continuously, 3.0kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1h, and the stirring reaction was continued for 1h under constant temperature after the addition was completed; 0.06kg oxalic acid was added to adjust the pH value to 4.6, and the stirring was continued for 1h; then, 0.4kg N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane was slowly added at 60°C for modification, and the stirring was continued for 1h after the addition was completed to make the reaction more fully; finally, the slurry was filtered and washed, and the slurry was dried at 100°C to obtain a modified calcium aluminum phosphosilicate antirust pigment product.
[0039] Embodiment 5:
[0040] 1.5kg potassium silicate, 1.2kg aluminum citrate, 1.6kg calcium nitrate and 5.5kg water were added into the reactor, the stirring speed was 200r / min, and the mixture was stirred for 0.5h to obtain a slurry; the slurry was heated to 80°C and stirred continuously, 4.8kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5h. After the addition was completed, the reaction was continued under constant temperature stirring for 1h; 0.22kg citric acid was added to adjust the pH value to 4.1, and the reaction was continued under constant temperature stirring for 1h; then, the temperature was lowered to 60°C, and 0.4kg γ-(2,3-epoxypropoxy)propyltrimethoxysilane was slowly added for modification, and the reaction was continued for 1h after the addition was completed to make the reaction more complete; finally, the mixture was filtered, washed, and dried at 90°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0041] Embodiment 6:
[0042] 1.6kg calcium silicate, 0.8kg sodium aluminate, 1.5kg calcium citrate and 5.0kg water were added into the reactor, stirred at a speed of 200r / min, stirred for 0.5h to obtain slurry; the slurry was heated to 50°C, stirred continuously, 4.8kg industrial phosphoric acid was taken, prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5h, and the stirring reaction was continued at a constant temperature for 1h after the addition was completed; 0.20kg tartaric acid was added to adjust the pH value to 4.7, and the stirring was continued for 1.5h; then, 0.3kg vinyltrimethoxysilane was slowly added for modification, and the stirring was continued for 1h after the addition was completed to make the reaction more fully; finally, the mixture was filtered, washed, and dried at 80°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0043] Example 7
[0044] 1.1 kg magnesium silicate, 3.0 kg pseudo-boehmite, 1.2 kg calcium oxalate and 5.5 kg water were added into the reactor, stirred at a speed of 200 r / min, stirred for 0.5 h to obtain a slurry; the slurry was heated to 50°C, stirred continuously, 4.9 kg industrial phosphoric acid was taken, prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5 h, and the stirring reaction was continued at a constant temperature for 1 h after the addition was completed; 0.12 kg malic acid was added to adjust the pH value to 4.4, and the stirring was continued for 2 h; then, 0.45 kg γ-aminopropyltrimethoxysilane was slowly added for modification, and the stirring was continued for 1 h after the addition was completed to make the reaction more fully proceed; finally, the mixture was filtered, washed, and dried at 55°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0045] Example 8
[0046] 1.0kg silicon dioxide, 0.5kg lithium silicate, 2kg aluminum acetate, 0.5kg calcium tartrate and 4.5kg water were added into the reactor, the stirring speed was 200r / min, and the stirring was continued for 0.5h to obtain slurry; the slurry was heated to 50°C and stirred continuously, 4.2kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1.5h, and the stirring reaction was continued for 1h under constant temperature after the addition was completed; 0.22kg succinic acid was added to adjust the pH value to 4.9, and the stirring was continued for 1h; then, 0.4kg γ-methacryloxypropyltrimethoxysilane was slowly added for modification, and the stirring was continued for 1h after the addition was completed to make the reaction more fully; finally, the mixture was filtered, washed, and dried at 70°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0047] Example 9
[0048] 1.2kg potassium silicate, 0.8kg aluminum citrate, 0.8kg sodium aluminate, 1.0kg calcium nitrate, 0.3kg calcium oxide and 5.0kg water were added into the reactor, the stirring speed was 200r / min, and the mixture was stirred for 0.5h to obtain a slurry; the slurry was heated to 85°C and stirred continuously, 3.9kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was added dropwise into the slurry for 1h, and the stirring reaction was continued for 1h under constant temperature after the addition was completed; 0.05kg citric acid and 0.1kg lactic acid were added to adjust the pH value to 4.1, and the stirring was continued for 1h; then, the temperature was lowered to 60°C, and 0.39kg γ-methacryloxypropyltrimethoxysilane was slowly added for modification, and the stirring was continued for 1h after the addition was completed to make the reaction more fully; finally, the mixture was filtered, washed, and dried at 90°C to obtain a modified calcium aluminum phosphosilicate antirust pigment.
[0049] Example 10
[0050] 0.8kg strontium silicate, 0.6kg magnesium silicate, 1.0kg aluminum citrate, 1.6kg calcium nitrate and 4.5kg water were added into the reactor, the stirring speed was 200r / min, and the stirring was continued for 0.5h to obtain a slurry; the slurry was heated to 45°C and stirred continuously, 3.7kg industrial phosphoric acid was taken and prepared into a 30% aqueous solution, and then the phosphoric acid solution was dripped into the slurry for 1h, and the stirring reaction was continued for 1h under constant temperature after the dripping was completed; 0.1kg tartaric acid and 0.08kg malic acid were added to adjust the pH value to 4.3, and the stirring was continued for 2h; then, the temperature was raised and 0.28kg vinyl tris-(2-methoxyethoxy)-silane was slowly added at 60°C for modification, and the stirring was continued for 1h after the addition was completed to make the reaction more fully; finally, the modified calcium aluminum phosphosilicate antirust pigment was obtained by filtering and washing, and drying at 100°C.
[0051] Comparative Example 1
[0052] 60 parts of calcium aluminum phosphate were surface treated with 0.2 parts of triethanolamine, then coated and deposited with 10 parts of nano-Al2(SiO3)3 and 10 parts of nano-CaSiO3, and finally 21 parts of fillers (including 8 parts of BaSO4, 6 parts of talc, and 7 parts of kaolin) were added, and the reaction temperature was controlled at 60°C for 4 hours. After the reaction, the mixture was filtered, washed, dried, and precipitated, and finally crushed by air flow to less than 5um to obtain calcium aluminum phosphosilicate antirust pigment.
[0053] Application Example 1
[0054] The modified calcium aluminum phosphosilicate antirust pigment prepared in Example 1, the calcium aluminum phosphosilicate antirust pigment prepared in Comparative Example 1, zinc phosphate, and modified aluminum tripolyphosphate were applied to waterborne acrylic paints for performance comparison tests. The modified aluminum tripolyphosphate and zinc phosphate used as comparisons are both antirust pigment products produced by Guangxi Xinjing Technology Co., Ltd. and sold on the market.
[0055] Preparation of water-based acrylic anticorrosive coating: First, 58% water-based acrylic resin, 12% water, 0.4% additives, 0.8% pH regulator, 8% antirust pigment, and 20% filler are fully mixed and dispersed uniformly according to mass fraction to make slurry, and grinding media is added to grind to a certain fineness, and then the remaining 0.8% additives are added after sieving and fully stirred to obtain water-based acrylic anticorrosive coating. The additives are dispersant, defoamer, film-forming additive, substrate wetting agent, and thickener, with a weight ratio of 2.5:1:1.4:1:1.2, the pH regulator is AMP-95, and the filler is sericite, barium sulfate, and titanium dioxide with a weight ratio of 1:1:0.9.
[0056] According to HG / T 4758-2014 water-based acrylic resin coating, storage stability, adhesion, anti-rust performance and other tests were carried out. The test results are shown in Table 1 and Figure 3 .
[0057] From Table 1 and Figure 3 It can be seen that the modified aluminum tripolyphosphate in the water-based acrylic anti-corrosion coating has poor compatibility and stability with the resin and poor use effect. The modified calcium aluminum phosphosilicate anti-rust pigment of the present invention has good compatibility with water-based acrylic acid. The obtained water-based acrylic anti-corrosion coating has good thermal stability and strong adhesion. At the same time, the salt spray anti-rust performance is significantly better than that of zinc phosphate.
[0058] Table 1 Performance index of water-based acrylic coating
[0059]
[0060] Application Example 2
[0061] The modified calcium aluminum phosphosilicate antirust pigment, zinc phosphate, and modified aluminum tripolyphosphate prepared in Example 2 were applied to waterborne epoxy resin coatings for performance comparison tests. The modified aluminum tripolyphosphate and zinc phosphate used as comparisons are both antirust pigment products produced by Guangxi Xinjing Technology Co., Ltd. and sold on the market.
[0062] Paint making: 55% waterborne epoxy resin, 16% water, 0.5% additive, 0.5% pH adjuster, 8% anti-rust pigment, and 19% filler are first mixed and dispersed evenly by mass fraction to make a slurry, and then grinding media is added to grind to a certain fineness. After sieving, the remaining 1% of additive is added and stirred to obtain a finished waterborne epoxy resin anticorrosive paint. The additives are dispersant, defoamer, cosolvent, substrate wetting agent, and thickener in a weight ratio of 3:1:1.5:1:1.5, the pH adjuster is triethanolamine, and the filler is talcum powder, barium sulfate, and titanium dioxide in a weight ratio of 1:1.2:1.
[0063] According to HG / T 4759-2014 waterborne epoxy resin anticorrosive coating, storage stability, adhesion, anti-rust performance and other tests were carried out. The results are shown in Table 2 and Figure 4 .
[0064] From Table 2 and Figure 4 It can be seen that the modified calcium aluminum phosphosilicate antirust pigment of the present invention has good storage stability and strong adhesion in a waterborne epoxy resin system, and its salt spray antirust performance is better than that of modified aluminum tripolyphosphate and zinc phosphate.
[0065] Table 2 Waterborne epoxy resin anticorrosive coating
[0066]
[0067] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A phosphosilicate anti-rust pigment, characterized in that: The method comprises the following raw materials in parts by weight: 60 to 100 parts of phosphoric acid, 20 to 40 parts of silicon source, 10 to 70 parts of aluminum source, 10 to 70 parts of calcium source, 1 to 10 parts of pH regulator, and 1 to 10 parts of modifier; the method for preparing the phosphosilicate antirust pigment comprises the following steps: (1) weighing a silicon source, an aluminum source and a calcium source, adding deionized water in an amount of 1 to 2 times the total mass of the silicon source, the aluminum source and the calcium source, stirring and mixing at a certain speed to make a uniformly dispersed slurry; (2) Weigh phosphoric acid to prepare an aqueous solution with a mass percentage concentration of 25 to 50%, and dropwise add the phosphoric acid solution to the slurry at a temperature of 40 to 95° C. under stirring; after the phosphoric acid solution is added, adjust the pH of the slurry to 4 to 5 with a pH adjuster, and continue stirring the reaction under constant temperature conditions; (3) adjusting the slurry temperature of step (2) to 40-70° C., adding a modifier, and continuing to stir the reaction under constant temperature conditions; (4) filtering, washing and drying the slurry obtained in step (3) to obtain a modified calcium aluminum phosphosilicate antirust pigment.
2. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: The silicon source is one or more mixtures of silicon dioxide, silica sol, potassium silicate, sodium silicate, calcium silicate, magnesium silicate, lithium silicate, strontium silicate and ammonium silicate.
3. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: The aluminum source is one or a mixture of two or more of aluminum oxide, aluminum hydroxide, aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum carbonate, aluminum citrate, sodium aluminate, pseudo-boehmite, isopropoxy aluminum, and aluminum acetate.
4. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: The calcium source is one or a mixture of two or more of calcium oxide, calcium hydroxide, calcium carbonate, calcium oleate, calcium nitrate, calcium sulfate, calcium chloride, calcium oxalate, calcium citrate and calcium tartrate.
5. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: The pH regulator is one or a mixture of two or more of acetic acid, oxalic acid, citric acid, tartaric acid, malic acid, succinic acid, and lactic acid, and the modifier is vinyl silane, amino silane, or methacryloxy silane.
6. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: In the step (1), the rotation speed is 120-250 r / min, and the stirring time is 0.5-1 h; in the step (2), the stirring speed is 120-250 r / min, and the stirring reaction time is continued for 0.5-1.5 h.
7. The phosphosilicate anti-rust pigment according to claim 1, characterized in that: In the step (3), the stirring reaction time is 0.5 to 2 hours; in the step (4), the drying temperature is 55 to 120°C.
8. Use of the phosphosilicate anti-rust pigment according to any one of claims 1 to 7 in water-based paint.
9. The use according to claim 8, characterized in that: The water-based paint is a water-based epoxy resin paint or a water-based acrylic paint.