Ultrasonic surgical knife head and preparation method thereof

Through ultrasonic magnetorheological composite polishing, non-equilibrium magnetron sputtering and deep hot and cold treatment technology, an excellent composite DLC coating was prepared, which solved the problem of difficult to take into account the friction coefficient and thermal conductivity of the ultrasonic scalpel head, and significantly improved the The service life of the blade head and reduces production costs.

CN115679256BActive Publication Date: 2024-11-08HUNAN HANDLIKE MINIMALLY INVASIVE SURGERY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211223475.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-08
Publication Date
2024-11-08
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

The existing ultrasonic scalpel tip coating is difficult to achieve low friction coefficient, good hydrophobicity and high thermal conductivity at the same time, resulting in easy breakage of the cutting head and tissue eschar adhesion, affecting the surgical effect, and increasing medical costs with one-time use.

Method used

Using ultrasonic magnetorheological composite polishing, non-equilibrium magnetron sputtering and deep hot and cold treatment technology, a composite DLC coating with good finish, suitable sp2 and sp3 ratios, and small residual stress was prepared to reduce the friction coefficient of the cutting head and Improve its thermal conductivity.

Benefits of technology

It significantly improves the service life of ultrasonic scalpels, has 50% better performance than the existing technology, has simple process, is easy to mass production, reduces costs, and meets the needs of cutting head coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115679256B_ABST
    Figure CN115679256B_ABST
Patent Text Reader

Abstract

The invention discloses an ultrasonic surgical knife head and a preparation method thereof. The synergistic effect of ultrasonic magnetorheological composite polishing, unbalanced magnetron sputtering and deep cold heat treatment technology is adopted to prepare a knife head DLC coating microstructure with good smoothness, suitable sp2 and sp3 phase ratio and small residual stress. This invention breaks through the preparation technology of ultrasonic surgical knife head coating, greatly improves the service life of the ultrasonic surgical knife, and has simple process, low cost and easy mass production, which can well meet the demand for ultrasonic surgical knife head coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a blade coating and a preparation method thereof, in particular to an ultrasonic surgical blade and a preparation method thereof, and belongs to the technical field of medical device processing. Background Art

[0002] Ultrasound refers to sound waves with a frequency greater than 20kHz. Due to its good directionality and strong penetrating power, it has been widely used in many medical fields such as ultrasonic scalpel surgery, ultrasonic atomization, B-ultrasound examination, ultrasonic pharmaceutical manufacturing, etc. Compared with traditional surgery, ultrasonic scalpel surgery has the advantages of high cutting accuracy, small trauma range, good coagulation effect, clearer field of vision, greatly shortened operation time, and fast postoperative recovery, which brings great benefits to both doctors and patients.

[0003] The ultrasonic scalpel surgical system mainly consists of two parts: a high-frequency power source and an ultrasonic vibration system. The ultrasonic vibration system includes three parts: a transducer, a knife rod, and a knife head. Among them, the transducer is a device for energy conversion. It converts the oscillating electrical signal generated by the ultrasonic generator into a mechanical vibration signal, that is, converts electrical energy into mechanical energy and transmits it to the knife rod. The knife rod transmits high-frequency vibration (ultrasound) to the knife head. The knife head contacts the tissue and cuts the tissue by mechanical impact, accompanied by heat generation to achieve coagulation and hemostasis. During the working process, the knife head generates a lot of heat due to high-frequency friction, causing its temperature to increase significantly (up to 500°C). On the one hand, excessively high temperature will reduce the yield strength and fatigue limit of the ultrasonic scalpel, and the knife head is prone to breakage. On the other hand, tissue eschar adhesion will occur, affecting the surgical effect. Therefore, the knife head needs a low friction coefficient, good hydrophobicity, and a high thermal conductivity. Nowadays, ultrasonic scalpels are generally disposable, that is, the clinical practice adopts the measure of "disposable after one use". Although this ensures the safety of the operation, it increases the cost of the operation and reduces the patient's choice. At the same time, it wastes materials, increases manufacturing costs, and increases the economic burden on patients. These factors restrict the clinical promotion of ultrasonic scalpels. Therefore, coating the surface of the ultrasonic scalpel with a protective coating with low friction coefficient, good hydrophobicity and high thermal conductivity has become a common method to extend the service life of the blade.

[0004] Huang Renzhu of Jiangxi Medishi Technology Co., Ltd. provides a preparation method and application of an anti-adhesion surgical blade coating for a laser surgical system (publication number: CN112957541A), including the steps of: coating an oxidant manganese dioxide layer on the surgical blade, and then vacuum coating a multi-layer aluminum oxide layer, each aluminum oxide layer having a thickness of 200-600nm; wherein coating the surgical blade with a manganese dioxide layer includes the steps of: ultrasonically cleaning the surgical blade with anhydrous ethanol and deionized water for 5-10 minutes in turn, then immersing the surgical blade in an aqueous solution of manganese chloride, standing for 2-3 hours, taking out, washing and drying; then immersing the surgical blade in an ethanol solution of stearic acid, standing for 3-6 hours, taking out, rinsing with anhydrous ethanol, and then drying at 60-80°C for 1-2 hours. Li Mingshou disclosed a surgical knife with a built-in heating unit (publication number: CN107595379A), comprising a blade consisting of a blade body and a cutting part, an anti-adhesion structure is prepared on the surface of the blade, the anti-adhesion structure is one or two of the raised parts and recessed parts periodically distributed on the surface of the blade, and a hard coating with a hardness greater than the blade material is deposited on the surface of the blade to protect the anti-adhesion structure on the surface of the blade, and the hard coating is one of silicon carbide, beryllium oxide, aluminum nitride, and diamond. Liao Bin of Beijing Normal University disclosed a method for preparing a hydrophobic DLC coating (publication number: CN108677142A), comprising the following steps: 1S: using a gas ion source to perform high and low energy alternating cleaning on the substrate surface; 2S: using a carbon target as a cathode, using a Kaisao arc magnetic filtration deposition method to deposit a hydrophobic DLC coating on the substrate. This method is based on the Kaisao arc magnetic filtration deposition method. During the deposition process, carbon nanoclusters can be formed by themselves, and nano-concave-convex structures can be formed at the same time, which greatly reduces the preparation cost and greatly improves the binding force of the nanoparticles themselves. The hydrophobic DLC coating produced by this method has the characteristics of good hydrophobicity and non-wetting. The high-frequency scalpel produced is wear-resistant, non-sticky, and blood is dispersed without agglomeration, which improves the key problem of blood agglomeration affecting the doctor's vision during surgery, thereby improving the working conditions of medical staff.

[0005] However, these thin film preparation processes all have their own limitations, and it is difficult to obtain thin film materials with good comprehensive properties such as low friction coefficient, good hydrophobicity and high thermal conductivity. At the same time, from the above information, it can be seen that the current research on scalpel coatings mainly focuses on the selection of coating materials and the optimization of coating processes, and there is no report on the influence of the microstructure of coating materials on the service performance of ultrasonic scalpels. However, the microstructure of coating materials such as roughness, phase composition, residual stress, thickness, etc. directly determines the physical properties of the coating, which in turn affects the service performance of ultrasonic scalpels. Diamond-like amorphous carbon film (DLC) is composed of sp2 and sp3 carbon-carbon chemical bonds. Due to its combination of the dual characteristics of carbon group elements and diamond-like structure, such as high hardness and elastic modulus, small friction coefficient, good biocompatibility, excellent insulation performance and light transmittance, it has broad application prospects and development potential in mechanical electronics, semiconductors, biomedicine and other directions with relatively large surface treatment requirements. Summary of the invention

[0006] In order to improve the service performance of an ultrasonic scalpel by controlling the microstructure of a composite DLC coating, the present invention provides an ultrasonic scalpel head and a preparation method thereof, wherein ultrasonic magnetorheological composite polishing, unbalanced magnetron sputtering and heat treatment technology are used to prepare a coating microstructure with good smoothness, a suitable sp2 and sp3 phase ratio, and small residual stress, thereby greatly reducing the friction coefficient of the head and improving its thermal conductivity, thereby increasing the service life of the ultrasonic scalpel.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] An ultrasonic surgical knife head, characterized in that it comprises a head substrate, a transition layer and a DLC layer;

[0009] The chemical composition of the substrate is one of TC4, TC9 and TC11; the chemical composition of the transition layer is one of Ni, Au and Al; the chemical composition of the DLC layer is one of N-DLC, B-DLC and F-DLC;

[0010] The substrate roughness Ra is 20 to 60 nm;

[0011] The thickness of the transition layer is 0.5 to 1 micron;

[0012] The thickness of the DLC layer is 2 to 4 microns;

[0013] The content of sp2 bonds in the DLC layer is 50% to 70%, and the content of sp3 bonds is 20% to 40%.

[0014] As a preferred embodiment, the ultrasonic surgical blade head of the present invention is characterized in that the microstructure of the substrate includes α phase and β phase; the average grain size of the α phase is 2 to 5 microns.

[0015] As a preferred embodiment, the present invention provides an ultrasonic surgical knife head, characterized in that the thermal conductivity of the knife head is 3 to 7 W / (m·K); and the friction coefficient of the knife head is 0.1 to 0.3.

[0016] The present invention provides a method for preparing an ultrasonic surgical knife head, characterized by comprising the following steps:

[0017] S1. Pretreatment: First, grind and polish the surface of the cutter head substrate, then use acetone and alcohol to ultrasonically clean the substrate in turn, and finally blow dry for standby use. The polishing method is ultrasonic magnetorheological composite polishing, the ultrasonic frequency is 20-30kHz, the output amplitude is 5-10 microns, the magnetic induction intensity is 1000-2000Gs, and the tool head speed is 200-300r / min;

[0018] S2. Cleaning and Activation: Place the blow-dried blade substrate on the workpiece rotating bracket in the coating chamber, evacuate the reaction chamber to a vacuum degree of less than 10 -5 When Pa, argon gas is introduced, and the ion source is turned on for sputtering to clean and activate the surface of the workpiece and the target material;

[0019] S3, deposition of transition layer: after sputtering and cleaning, a transition layer is deposited on the surface of the tool head substrate by using a DC magnetron sputtering method using one of the metal target materials Ni, Au and Al;

[0020] S4, depositing a DLC layer: after depositing the transition layer, a DLC layer is deposited on the metal transition layer by using a reactive magnetron sputtering method, using a graphite target and nitrogen, a boron target, and carbon tetrafluoride gas;

[0021] S5. Cryogenic heat treatment: After the DLC layer is deposited, the product is placed in a cryogenic furnace for cryogenic treatment to obtain the finished product.

[0022] As a preferred embodiment, the present invention provides a method for preparing an ultrasonic surgical blade tip, characterized in that in the cleaning and activation process, the sputtering power used is 100 to 300 W, the negative bias voltage is -200 to -100 V, and the sputtering time is 10 to 30 min.

[0023] As a preferred embodiment, the present invention provides a method for preparing an ultrasonic surgical knife tip, characterized in that in the process of depositing the transition layer, high-purity argon is used as the ionizing gas, the sputtering power used is 300 to 500 W, the negative bias voltage is -200 to -50 V, and the sputtering time is 0.5 to 1 h.

[0024] As a preferred embodiment, the present invention provides a method for preparing an ultrasonic surgical knife head, characterized in that in the process of depositing the DLC layer, high-purity argon is used as a protective and ionizing gas, the sputtering power used is 200 to 600 W, the negative bias voltage is -300 to 0 V, and the sputtering time is 1 to 4 hours.

[0025] As a preferred embodiment, the present invention provides a method for preparing an ultrasonic surgical knife tip, characterized in that, in the deep cold heat treatment, the medium is liquid nitrogen and the insulation time is 15 to 20 hours.

[0026] The present invention discloses an ultrasonic surgical knife head and a preparation method thereof, wherein the service life of the ultrasonic surgical knife is ≥4 hours.

[0027] Principles and advantages

[0028] The present invention has made a breakthrough in the preparation technology of ultrasonic surgical blade tip coating, and for the first time, through the synergistic effect of ultrasonic magnetorheological composite polishing, unbalanced magnetron sputtering and deep cold heat treatment technology, a coating microstructure corresponding to the service life of an excellent ultrasonic surgical blade is prepared.

[0029] During surgery, the ultrasonic scalpel blade is easily adhered to substances including coagulants, proteins, blood, tissue particles and other component fluids. The accumulation of these substances will increase the impedance of the blade and reduce the cutting and coagulation performance of the blade. In order to compensate for the increase in impedance, the generator provides an increasing amount of power to the blade to continue working until the power delivered by the generator exceeds a predetermined threshold, at which time the generator is turned off or enters a "locked" state. When the generator enters the locked state, the surgical operation is interrupted or stopped due to a fault. Therefore, the blade coating material should have high thermal conductivity, low friction coefficient and good biocompatibility. These physical properties of the coating are closely related to its tissue structure. The following will analyze the relationship between roughness, phase composition and residual stress and the friction coefficient and thermal conductivity of the coating one by one, and obtain the ideal microstructure through the optimization of the preparation process.

[0030] The relationship between roughness and friction coefficient. The friction coefficient refers to the ratio of the friction force between two surfaces to the vertical force acting on one of the surfaces. The smaller the friction coefficient, the better the lubricity of the coating. The friction coefficient of the coating is related to the surface roughness of the material. The friction coefficient increases with the increase of surface roughness. During the sliding friction process of the surface with large roughness, the micro-convex bodies on the surfaces of the two contacting bodies will undergo a violent mechanical interlocking phenomenon, thereby increasing the friction coefficient. When the roughness decreases, the coating particles are more compact, which can significantly reduce the friction coefficient. Therefore, controlling the roughness of the coating is one of the methods to reduce the friction coefficient. The surface of the tool head after processing is rough, and the surface finish needs to be improved through a polishing process. Due to the complex structure of the tool head and the large number of concave surfaces, traditional polishing processes such as mechanical polishing are difficult to handle. The present invention adopts ultrasonic magnetorheological composite polishing. In this process, a polishing tool head with a small diameter is used, and the end face of the polishing tool head is used for polishing. During the polishing process, after the workpiece is correctly clamped, magnetorheological fluid is introduced into the rotating polishing tool head, and a magnetic field with a certain magnetic induction intensity is applied, so that the magnetorheological fluid forms a flexible polishing tool with a certain removal ability on the end face of the polishing tool head. At the same time, ultrasonic vibration is applied to the polishing tool, and the ultrasonic vibration energy directly acts on the polishing processing area to improve the polishing efficiency. This method can use a small-diameter polishing tool head, which can not only achieve nano-scale surface polishing of concave surfaces with a small curvature radius, but also can be extended to the polishing of free-form surfaces. The roughness of the complex concave surface structure is greatly reduced through ultrasonic magnetorheological composite polishing, and the friction coefficient of the coating is improved.

[0031] The relationship between phase composition and friction coefficient and thermal conductivity. DLC is composed of sp2 and sp3 carbon-carbon chemical bonds. The sp2 bond is a hybridization of a 2s orbital and two 2p orbitals, with a triangular plane and a bond angle of 120°. The sp3 bond is a hybridization of a 2s orbital and three 2p orbitals, with a regular tetrahedron and a bond angle of 109°. Carbon atoms are bonded to each other in the form of sp3 bonds (all σ bonds), which is diamond, and has high hardness, high thermal conductivity, good chemical stability, etc. Carbon atoms are bonded to each other in the form of sp2 bonds (σ+π bonds), which is graphite, and has low friction coefficient, self-lubrication, etc. Therefore, it can be seen that the more sp3 bonds there are, the more diamond phases there are in DLC, and the corresponding k value of phonon thermal conductivity is higher, so the thermal conductivity of DLC is greater. On the other hand, the more sp2 bonds there are, the more graphite phases there are in DLC, and the van der Waals force between adjacent graphite layers is weak, which makes it very easy to produce interlayer sliding, so that it has outstanding non-stick performance and friction coefficient, so the friction coefficient of DLC is smaller. The present invention deposits a transition layer and a DLC layer on the sample after cleaning and activation. In the process of technical development, an attempt was made to adopt only the scheme of depositing DLC ​​process, but no matter how it is optimized, the friction coefficient and thermal conductivity of the obtained coating are still not ideal. This is because the introduction of the transition layer is conducive to improving the bonding force of the DLC layer, reducing the number of defects, and improving the friction coefficient of the coating. On the other hand, the metal elements Ni, Au and Al with high thermal conductivity values ​​are also more conducive to improving the thermal conductivity of the coating. The present invention has determined the process parameters of depositing the transition layer and depositing the DLC layer through a large number of experiments. Under the above-mentioned process parameters, a phase content suitable for the ratio of sp2 and sp3 chemical bonds is obtained, which can well balance the contradictory relationship between the friction coefficient and thermal conductivity of the coating, and is conducive to the service life of the ultrasonic scalpel.

[0032] The relationship between residual stress and friction coefficient and thermal conductivity. As a new type of hard film material, DLC film has a series of excellent properties and is widely used in mechanical, electronic, optics, thermal, acoustic, medical and other fields. Residual stress is a very important factor affecting the bonding strength between the film and the substrate, which is divided into two categories: intrinsic stress and thermal stress. Studies have shown that although the existence of a certain amount of residual stress is beneficial to the bonding strength and other properties of the coating, excessive residual stress often reduces the adhesion between the film and the substrate, resulting in defects such as shedding, pores, and cracks during use, which in turn affects the friction coefficient and thermal conductivity of the coating.

[0033] The certain temperature generated during the coating process is the main source of residual stress in the DLC film. The inventors found that the deposition of the DLC film directly leads to an increase in the pressure of the substrate (about 20 to 40 MPa), indicating that the residual stress of the DLC film deposited on the ultrasonic scalpel tip is in a compressive stress state. Using a cryogenic treatment process, when the ambient temperature drops significantly, the volume of the substrate will shrink, and the compressive stress on the surrounding area will decrease, which can greatly reduce the residual stress (by about 50%). Therefore, the inventors adopted a cryogenic heat treatment process and found that when the heat treatment process is optimized, the friction coefficient and thermal conductivity of the resulting coating can be significantly improved, thereby achieving the purpose of increasing the service life of the ultrasonic scalpel.

[0034] Compared with the prior art, the advantages of the present invention are as follows:

[0035] 1) Excellent performance. Ultrasonic service life is 50% better than that of existing technologies;

[0036] 2) The process is simple. There are only two deposition steps;

[0037] 3) Easy to mass produce. The production efficiency is 2 to 3 times that of the existing technology.

[0038] In summary, the present invention adopts the synergistic effect of ultrasonic magnetorheological composite polishing, unbalanced magnetron sputtering and deep cold heat treatment technology to prepare a blade DLC coating microstructure with good smoothness, suitable sp2 and sp3 phase ratio, and small residual stress. It breaks through the preparation technology of ultrasonic scalpel blade coating, greatly improves the service life of ultrasonic scalpel, and has simple process, low cost, and easy mass production, which can well meet the needs of ultrasonic scalpel blade coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a scanning electron microscope photo of the coating microstructure.

[0040] Figure 2 is a scanning electron microscope photograph of the coating cross section.

[0041] Figure 3 It is the test result of substrate roughness.

[0042] Figure 4 This is the test result of coating XPS. DETAILED DESCRIPTION

[0043] The method of the present invention is further described below with reference to three examples.

[0044] Embodiment 1:

[0045] An ultrasonic surgical knife head and a preparation method thereof, wherein the process is as follows:

[0046] A. Pretreatment: First, the surface of the cutter head substrate is polished and treated with ultrasonic magnetorheological composite polishing. The ultrasonic frequency is 25kHz, the output amplitude is 5 microns, the magnetic induction intensity is 1500Gs, and the tool head speed is 200r / min. Then, the substrate is ultrasonically cleaned with acetone and alcohol in turn, and finally blown dry for standby use. The substrate roughness Ra is 29.5nm. Figure 3 ;

[0047] B. Cleaning and Activation: Place the blow-dried blade substrate on the workpiece rotating bracket in the coating chamber, and evacuate the reaction chamber to a vacuum degree of less than 10 -5 When the argon gas was introduced at 1.5 Pa, the ion source was turned on for sputtering, the sputtering power used was 150 W, the negative bias voltage was -100 V, and the sputtering time was 15 min to clean and activate the workpiece and target surface;

[0048] C. Deposition of transition layer: After sputtering and cleaning, a transition layer is deposited on the surface of the tool head substrate using a metal Cr target by DC magnetron sputtering. High-purity argon is used as the ionizing gas. The sputtering power is 400W, the negative bias voltage is -200V, the sputtering time is 0.5h, and the thickness of the transition layer is 0.8 microns. Figure 2 ;

[0049] D. Deposition of DLC layer: After the transition layer is deposited, a B-DLC layer is deposited on the metal transition layer using a graphite target and a boron target by reactive magnetron sputtering. High-purity argon is used as a protective and ionizing gas. The sputtering power used is 400 W, the negative bias voltage is -200 V, the sputtering time is 2 h, and the DLC layer thickness is 3.2 μm. Figure 2 ;

[0050] E. Cryogenic heat treatment: After depositing the DLC layer, the product is placed in a cryogenic furnace filled with liquid nitrogen for 20 hours for cryogenic treatment. The microstructure is as follows: Figure 1 ;

[0051] F. Organization and performance test: The results are as follows: The content of sp2 bonds in the DLC layer is 55%, and the content of sp3 bonds is 31%. Figure 4 (XPS uses a radiation source with an energy of 1000-1500eV, which can excite inner-layer electrons. Each element has its specific core energy, and the shift of this core energy reflects the chemical bonding situation at each position. The largest shift is caused by the Coulomb potential generated by the ions binding to nearby atoms. XPS measures the change in this displacement to measure the sp2 and sp3 content of the DLC film), the thermal conductivity of the DLC layer is 4W / (m·K), the friction coefficient of the DLC layer is 0.15, and the service life of the ultrasonic scalpel is 4.5h.

[0052] Embodiment 2:

[0053] An ultrasonic surgical knife head and a preparation method thereof, wherein the process is as follows:

[0054] A. Pretreatment: First, the surface of the cutter head substrate is polished and subjected to ultrasonic magnetorheological composite polishing. The ultrasonic frequency is 30kHz, the output amplitude is 6 microns, the magnetic induction intensity is 1500Gs, and the tool head speed is 250r / min. Then, the substrate is ultrasonically cleaned with acetone and alcohol in turn, and finally blown dry for standby use. The substrate roughness Ra is 25nm;

[0055] B. Cleaning and Activation: Place the blow-dried blade substrate on the workpiece rotating bracket in the coating chamber, and evacuate the reaction chamber to a vacuum degree of less than 10 -5 When the argon gas was introduced at 1.5 Pa, the ion source was turned on for sputtering, the sputtering power used was 150 W, the negative bias voltage was -100 V, and the sputtering time was 15 min to clean and activate the workpiece and target surface;

[0056] C. Deposition of transition layer: After sputtering and cleaning, a transition layer is deposited on the surface of the tool head substrate using a metal Ni target by DC magnetron sputtering. High-purity argon is used as the ionizing gas. The sputtering power is 350W, the negative bias voltage is -100V, the sputtering time is 0.6h, and the thickness of the transition layer is 1.0 micron.

[0057] D. Deposition of DLC layer: After the transition layer is deposited, a N-DLC layer is deposited on the metal transition layer using a graphite target and nitrogen by reactive magnetron sputtering. High-purity argon is used as a protective and ionizing gas. The sputtering power used is 500 W, the negative bias voltage is -100 V, the sputtering time is 1.5 h, and the DLC layer thickness is 3 μm.

[0058] E. Cryogenic heat treatment: After the DLC layer is deposited, it is placed in a cryogenic furnace filled with liquid nitrogen for 15 hours for cryogenic treatment to obtain the finished product;

[0059] F. Tissue performance test: The results are as follows: the content of sp2 bonds in the DLC layer is 60%, the content of sp3 bonds is 38%, the thermal conductivity of the DLC layer is 3.5 W / (m·K), the friction coefficient of the DLC layer is 0.12, and the service life of the ultrasonic scalpel is 5 h.

[0060] Embodiment 3:

[0061] An ultrasonic surgical knife head and a preparation method thereof, wherein the process is as follows:

[0062] A. Pretreatment: First, the surface of the cutter head substrate is polished and subjected to ultrasonic magnetorheological composite polishing. The ultrasonic frequency is 30kHz, the output amplitude is 6 microns, the magnetic induction intensity is 1500Gs, and the tool head speed is 250r / min. Then, the substrate is ultrasonically cleaned with acetone and alcohol in turn, and finally blown dry for standby use. The substrate roughness Ra is 25nm;

[0063] B. Cleaning and Activation: Place the blow-dried blade substrate on the workpiece rotating bracket in the coating chamber, and evacuate the reaction chamber to a vacuum degree of less than 10 -5 When the argon gas was introduced at 1.50 Pa, the ion source was turned on for sputtering, the sputtering power used was 100 W, the negative bias voltage was -100 V, and the sputtering time was 20 min to clean and activate the workpiece and target surface;

[0064] C. Deposition of transition layer: After sputtering and cleaning, a transition layer is deposited on the surface of the tool head substrate using a metal Ti target by DC magnetron sputtering. High-purity argon is used as the ionizing gas. The sputtering power is 400W, the negative bias voltage is -100V, the sputtering time is 0.5h, and the thickness of the transition layer is 0.6 microns.

[0065] D. Deposition of DLC layer: After the transition layer is deposited, a reactive magnetron sputtering method is used to deposit an F-DLC layer on the metal transition layer using a graphite target and carbon tetrafluoride gas. High-purity argon is used as a protective and ionizing gas. The sputtering power used is 500 W, the negative bias voltage is -200 V, the sputtering time is 2 h, and the DLC layer thickness is 3.5 μm.

[0066] E. Cryogenic heat treatment: After the DLC layer is deposited, it is placed in a cryogenic furnace filled with liquid nitrogen for 20 hours for cryogenic treatment to obtain the finished product;

[0067] F. Tissue performance test: The results are as follows: the content of sp2 bonds in the DLC layer is 58%, the content of sp3 bonds is 34%, the thermal conductivity of the DLC layer is 4 W / (m·K), the friction coefficient of the DLC layer is 0.12, and the service life of the ultrasonic scalpel is 5.5 h.

[0068] Comparative Example 1

[0069] The only difference from Example 3 is that a mechanical polishing method is used, the roughness is poor, the friction coefficient of the coating reaches 0.4, and the service life of the ultrasonic surgical knife is less than 2 hours.

[0070] Comparative Example 2

[0071] The only difference from Example 3 is that no transition layer is deposited, the coating has poor adhesion, pores, cracks, etc., and the service life of the ultrasonic surgical knife is less than 2 hours.

[0072] Comparative Example 3

[0073]

[0074]

[0075] Except for the conditions indicated above, other conditions are consistent with those in Example 3.

[0076] Comparative Example 4

[0077] The only difference from Example 3 is that the DLC layer is not doped, the residual stress is increased, and the friction coefficient reaches 0.3, and the service life of the ultrasonic surgical knife is less than 2 hours.

[0078] Comparative Example 5

[0079] The only difference from Example 3 is that no cryogenic treatment is performed, the residual stress is relatively large, the coating adhesion is relatively poor, the coating has fallen off, and the service life of the ultrasonic surgical knife is less than 1.5 hours.

[0080] The above-described examples are only preferred implementation methods of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. Other equivalent changes, modifications, substitutions and combinations made in accordance with the principles and contents of the present invention still fall within the scope of protection of the present invention.

Claims

1. A method for preparing a coating on an ultrasonic surgical blade head. It is characterized in that The invention comprises a tool head substrate, a transition layer and a DLC layer; the chemical composition of the substrate is one of TC4, TC9 and TC11; the chemical composition of the transition layer is one of Ni, Au and Al; the chemical composition of the DLC layer is one of N-DLC, B-DLC and F-DLC; the thermal conductivity of the tool head is 3 to 7 W·m -1 K -1 The friction coefficient of the cutter head is 0.1 to 0.3; comprising the following steps: S1. Pretreatment: First, the surface of the cutter head substrate is polished, and then the substrate is ultrasonically cleaned with acetone and alcohol in turn, and finally blown dry for standby use. The polishing method is ultrasonic magnetorheological composite polishing, the ultrasonic frequency is 20-30kHz, the output amplitude is 5-10 microns, the magnetic induction intensity is 1000-2000Gs, and the tool head speed is 200-300r / min; the roughness Ra of the substrate surface is 20-60nm; S2. Cleaning and Activation: Place the blow-dried blade substrate on the workpiece rotating bracket in the coating chamber, evacuate the reaction chamber to a vacuum degree of less than 10 -5 When Pa, argon gas is introduced, and the ion source is turned on for sputtering to clean and activate the surface of the workpiece and the target material; S3, deposition of transition layer: after sputtering and cleaning, a transition layer is deposited on the surface of the tool head substrate by using a DC magnetron sputtering method using one of the metal target materials Ni, Au and Al; the thickness of the transition layer is 0.5 to 1 micron; S4, depositing a DLC layer: after depositing the transition layer, a DLC layer is deposited on the metal transition layer by using a graphite target and nitrogen, a boron target, and carbon tetrafluoride gas by reactive magnetron sputtering; the thickness of the DLC layer is 2 to 4 microns; the content of sp2 bonds in the DLC layer is 50% to 70%, and the content of sp3 bonds is 20 to 40%; S5. Cryogenic heat treatment: After the DLC layer is deposited, the product is placed in a cryogenic furnace for cryogenic treatment to obtain the finished product.

2. A method for preparing an ultrasonic surgical blade coating according to claim 1, It is characterized in that In the cleaning and activation process, the sputtering power used is 100 to 300 W, the negative bias voltage is -200 to -100 V, and the sputtering time is 10 to 30 minutes.

3. The method for preparing a coating on an ultrasonic surgical blade according to claim 1, It is characterized in that In the process of depositing the transition layer, high-purity argon is used as the ionized gas, the sputtering power used is 300 to 500 W, the negative bias voltage is -200 to -50 V, and the sputtering time is 0.5 to 1 hour.

4. The method for preparing a coating on an ultrasonic surgical blade according to claim 1, It is characterized in that In the process of depositing the DLC layer, high-purity argon is used as a protective and ionizing gas, the sputtering power used is 200 to 600 W, the negative bias voltage is -300 to 0 V, and the sputtering time is 1 to 4 hours.

5. The method for preparing a coating on an ultrasonic surgical blade according to claim 1, It is characterized in that In the deep cold heat treatment, the medium is liquid nitrogen and the insulation time is 15 to 20 hours.

6. A method for preparing an ultrasonic surgical blade coating according to any one of claims 1 to 5, Features: The service life of ultrasonic surgical knife is ≥4h.

7. The method for preparing a coating on an ultrasonic surgical blade according to claim 1, It is characterized in that The microstructure of the substrate includes α phase and β phase; the average grain size of the α phase is 2 to 5 microns.

Citation Information

Patent Citations

  • Scalpel with built-in heating unit

    CN107595379A

  • Method for producing hydrophobic DLC coating layer

    CN108677142A

  • Preparation method and application of anti-adhesion scalpel head coating of laser surgical system

    CN112957541A

  • Method for improving bonding strength of interface between hard coating and substrate

    CN102517539A

  • Corrosion and abrasion resistant Cr-DLC coating for aluminum alloy surface and preparation methods of Cr-DLC coating

    CN105525258A