Lithium ion conductive solid electrolyte and all-solid-state battery

By adopting specific crystal structures and stoichiometric formulas in oxide-based solid electrolytes and combining low-temperature sintering technology, the problem that it is difficult for oxide-based solid electrolytes to achieve sufficient ion conductivity and density at low temperatures is solved, and high-efficiency full-scale Solid battery performance and economy.

CN115699213BActive Publication Date: 2024-11-05RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180041258.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-10
Filing Date
2021-06-09
Publication Date
2024-11-05
Estimated Expiration
2041-06-09

AI Technical Summary

Technical Problem

It is difficult for oxide-based solid electrolytes to achieve sufficient ion conductivity and relative density during low-temperature sintering, which affects the performance of all-solid batteries.

Method used

Lithium-ion conductive solid electrolyte with crystal structures based on LiTa2PO8, LiTa3O8, Ta2O5, and TaPO5 is prepared by using a solid electrolyte with high relative density and ion conductivity through specific stoichiometric formulas and elements, combined with low-temperature sintering technology.

Benefits of technology

It realizes the preparation of lithium-ion conductive solid electrolytes with high ion conductivity and relative density at low temperatures, improves the economy and performance stability of all-solid batteries, inhibits the decomposition or deterioration of positive or negative electrode materials, and ensures sufficient Ion conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003987692550000281
    Figure BDA0003987692550000281
  • Figure HDA0003987692560000011
    Figure HDA0003987692560000011
Patent Text Reader

Abstract

One technical solution of the present invention relates to a lithium ion conductive solid electrolyte or an all-solid battery, wherein the lithium ion conductive solid electrolyte satisfies any one of (I) to (III). (I) having a crystal structure based on LiTa2PO8 and a crystal structure based on at least one compound selected from LiTa3O8, Ta2O5 and TaPO5; (II) having a stoichiometric formula Li a1 Ta b1 B c1 P d1 O e1 [0.5<a1<2.0、1.0<b1≤2.0、0<c1<0.5、0.5<d1<1.0、5.0<e1≤8.0] represents (III) by the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 [0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge].
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One technical solution of the present invention relates to a lithium ion conductive solid electrolyte or an all-solid-state battery. Background Art

[0002] In recent years, there has been a growing demand for high-output, high-capacity batteries as power sources for laptop computers, tablet computers, mobile phones, smartphones, and electric vehicles (EVs). Among these, all-solid-state batteries, which use solid electrolytes instead of liquid electrolytes such as organic solvents, have attracted significant attention as they offer superior charge and discharge efficiency, charging speed, safety, and productivity.

[0003] As the solid electrolyte, inorganic solid electrolytes have attracted attention, and oxide-based and sulfide-based solid electrolytes are mainly known as the inorganic solid electrolyte.

[0004] When using sulfide-based solid electrolytes, although they have the advantage of being able to produce batteries through methods such as cold pressing, they are unstable with respect to humidity and may produce harmful hydrogen sulfide gas. Therefore, the development of oxide-based solid electrolytes is being carried out from the perspective of safety and other aspects.

[0005] As such an oxide-based solid electrolyte, Non-Patent Document 1 describes that LiTa2PO8 having a monoclinic crystal structure exhibits high lithium ion conductivity (total conductivity (25°C): 2.5×10 -4 S cm -1 ).

[0006] Prior art literature

[0007] Non-patent literature 1: J. Kim et al., J. Mater. Chem. A, 2018, 6, p22478-22482 Summary of the Invention

[0008] Problems to be solved by the invention

[0009] The grain boundary resistance of oxide-based solid electrolytes is extremely high. In order to obtain ion conductivity that can be used in all-solid-state batteries, it is necessary not only to pressurize the solid electrolyte powder into a mold but also to sinter it to make a high-density solid electrolyte.

[0010] During this sintering, from the perspectives of economy and equipment, it is expected that a solid electrolyte with sufficient ion conductivity and relative density can be obtained even if the sintering is carried out at a low temperature (for example, below 900°C). However, even when LiTa2PO8 described in non-patent document 1 is sintered at a low temperature, a solid electrolyte with a sufficiently high balance between ion conductivity and relative density cannot be obtained.

[0011] One aspect of the present invention is to provide a lithium ion conductive solid electrolyte having sufficient ion conductivity and relative density even when the firing temperature during the production of the solid electrolyte is set to a low temperature (for example, 900° C. or lower).

[0012] Means for solving problems

[0013] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned problems can be solved according to the following technical configuration examples, thereby completing the present invention.

[0014] The technical configuration examples of the present invention are as follows.

[0015] [1] A lithium ion conductive solid electrolyte having:

[0016] Based on the crystal structure of LiTa2PO8; and

[0017] Based on the crystal structure of at least one compound selected from LiTa3O8, Ta2O5 and TaPO5.

[0018] [2] A lithium ion conductive solid electrolyte composed of the stoichiometric formula Li a1 Ta b1 B c1 P d1 O e1 [0.5<a1<2.0, 1.0<b1≤2.0, 0<c1<0.5, 0.5<d1<1.0, 5.0<e1≤8.0] indicates.

[0019] [3] A lithium ion conductive solid electrolyte composed of the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 [0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge].

[0020] [4] The lithium ion conductive solid electrolyte according to any one of [1] to [3], wherein the content of tantalum element is 10.6 to 16.6 atomic %.

[0021] [5] The lithium ion conductive solid electrolyte according to any one of [1] to [4], wherein the phosphorus content is 5.3 to 8.3 atomic %.

[0022] [6] The lithium ion conductive solid electrolyte according to any one of [1] to [5], wherein the content of lithium element is 5.0 to 20.0 atomic %.

[0023] [7] The lithium ion conductive solid electrolyte according to any one of [1] to [6], comprising lithium, tantalum, phosphorus, and oxygen as constituent elements, and boron as a constituent element.

[0024] [8] The lithium ion conductive solid electrolyte according to any one of [1] to [7], comprising one or more elements Ma selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge as constituent elements.

[0025] [9] The lithium ion conductive solid electrolyte according to any one of [1] to [8], wherein the relative density, which is the percentage of the measured density calculated from the mass and volume of the lithium ion conductive solid electrolyte relative to the theoretical density of the crystal structure constituting the lithium ion conductive solid electrolyte, is 60% or more.

[0026]

[10] An all-solid-state battery comprising a positive electrode, a negative electrode and a solid electrolyte layer,

[0027] The positive electrode has a positive electrode active material,

[0028] The negative electrode has a negative electrode active material,

[0029] The solid electrolyte layer is located between the positive electrode and the negative electrode,

[0030] The solid electrolyte layer includes the lithium ion conductive solid electrolyte described in any one of [1] to [9].

[0031]

[11] The all-solid-state battery according to

[10] , wherein the positive electrode active material comprises LiM3PO4 [M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements of V and O], LiM5VO4 [M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti], Li2M6P2O7 [M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements of V and O], LiVP2O7, Li x7 V y7 M7 z7 [2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr], Li 1+x8 Al x8 M8 2-x8(PO4)3[0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge], LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiCoO2, LiNiO2, LiMn2O4, Li2CoP2O7, Li3V2(PO4)3, Li3Fe2(PO4)3, LiNi 0.5 Mn 1.5 O4 and Li4Ti5O 12 One or more compounds.

[0032]

[12] The all-solid-state battery according to

[10] or

[11] , wherein the negative electrode active material comprises LiM3PO4 [M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements of V and O], LiM5VO4 [M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti], Li2M6P2O7 [M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements of V and O], LiVP2O7, Li x7 V y7 M7 z7 [2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr], Li 1+x8 Al x8 M8 2-x8 (PO4)3[0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge], (Li 3-a9x9+(5-b9)y9 M9 x9 )(V 1-y9 M10 y9 )O4[M9 is one or more elements selected from Mg, Al, Ga and Zn, M10 is one or more elements selected from Zn, Al, Ga, Si, Ge, P and Ti, 0≤x9≤1.0, 0≤y9≤0.6, a9 is the average valence of M9, b9 is the average valence of M10], LiNb2O7, Li4Ti5O 12 、Li4Ti5PO 12 , TiO2, LiSi and graphite.

[0033]

[13] The all-solid-state battery according to any one of

[10] to

[12] , wherein the positive electrode and the negative electrode contain the lithium ion conductive solid electrolyte according to any one of [1] to [9].

[0034] Effects of the Invention

[0035] According to one embodiment of the present invention, even when the firing temperature during the production of the solid electrolyte is set to a low temperature (e.g., below 900°C), a solid electrolyte having sufficient ion conductivity and relative density can be obtained. Furthermore, by using the lithium ion conductive solid electrolyte material according to one embodiment of the present invention, it is possible to easily produce an all-solid-state battery that is economically efficient, suppresses the decomposition or deterioration of other materials such as the positive electrode or negative electrode material, and includes a solid electrolyte having sufficient ion conductivity while preventing short circuits in the positive electrode or negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 1 and 2 are XRD patterns of the solid electrolytes obtained in Examples 4 and 6 and Comparative Example 1. DETAILED DESCRIPTION

[0037] Lithium-ion conductive solid electrolytes

[0038] A lithium ion conductive solid electrolyte according to one embodiment of the present invention satisfies any one of the following requirements (I) to (III).

[0039] Requirement (I): Having a crystal structure based on LiTa2PO8 (hereinafter also referred to as "LTPO structure"), and a crystal structure based on at least one compound selected from LiTa3O8, Ta2O5 and TaPO5 (hereinafter also referred to as "impurity structure").

[0040] Requirement (II): According to the stoichiometric formula Li a1 Ta b1 B c1 P d1 O e1 [0.5<a1<2.0, 1.0<b1≤2.0, 0<c1<0.5, 0.5<d1<1.0, 5.0<e1≤8.0] indicates.

[0041] Requirement (III): According to the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 [0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge].

[0042] The lithium ion conductive solid electrolyte that satisfies the above requirement (I) is referred to as "the present solid electrolyte 1", the lithium ion conductive solid electrolyte that satisfies the above requirement (II) is referred to as "the present solid electrolyte 2", and the lithium ion conductive solid electrolyte that satisfies the above requirement (III) is referred to as "the present solid electrolyte 3".

[0043] Hereinafter, the present solid electrolytes 1 to 3 are also collectively referred to as “the present solid electrolyte”.

[0044] The present solid electrolyte 1 preferably satisfies the above requirement (II) or the above requirement (III).

[0045] The present solid electrolytes 2 and 3 preferably satisfy the above-mentioned requirement (I), respectively.

[0046] Whether the present solid electrolyte has the above-mentioned LTPO structure and impurity structure can be determined by X-ray diffraction (XRD) patterns, specifically by analyzing XRD patterns measured by the method described in the following Examples.

[0047] The solid electrolyte that satisfies the above-mentioned requirement (I) is specifically observed to have an XRD pattern in which a peak derived from the crystal structure of LiTa2PO8 described in non-patent document 1 is added to a peak derived from the crystal structure of at least one compound selected from LiTa3O8 (ICSD (Inorganic Crystal Structure Database) code: 493), Ta2O5 (ICSD code: 66366) and TaPO5 (ICSD code: 202041).

[0048] The crystallization rate of the LTPO structure of the present solid electrolyte (= crystallization amount of LTPO × 100 / total crystallization amount of all observed crystals) is preferably 60% or more, more preferably 70% or more, and further preferably 80% or more. The upper limit is not specifically limited and is less than 100%.

[0049] If the crystallinity of the LTPO structure of the present solid electrolyte is within the above range, the ion conductivity is high both within the crystal grains and at the grain boundaries, resulting in a tendency for the solid electrolyte to have high total ion conductivity and high relative density.

[0050] The crystallization ratio of the LTPO structure in the solid electrolyte can be calculated, for example, by performing Rietveld analysis on the obtained XRD pattern using the well-known analysis software RIETAN-FP (available from the homepage of the creator Fujio Izumi, "RIETAN-FP·VENUS System Distribution File" (http: / / fujioizumi.verse.jp / download / download.html)).

[0051] The crystallization rate of the impurity structure of the present solid electrolyte (= the crystallization amount of LiTa3O8, Ta2O5 and TaPO5 × 100 / the total crystallization amount of all observed crystals) is preferably 1% or more, more preferably 2% or more, preferably 40% or less, and more preferably 30% or less, from the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density.

[0052] The solid electrolyte 2 is composed of the stoichiometric formula Li a1 Ta b1 B c1 P d1 O e1 [0.5<a1<2.0、1.0<b1≤2.0、0<c1<0.5、0.5<d1<1.0、5.0<e1≤8.0] represents that the solid electrolyte 3 is composed of the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 [0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al, and Ge], thereby exerting the above-mentioned effect. When the present solid electrolyte 3 contains two or more elements Ma, the above c2 is the sum of all elements Ma.

[0053] The relative density of the present solid electrolyte is preferably 60% or higher, more preferably 70% or higher, and particularly preferably 80% or higher.

[0054] If the relative density is within the above range, it can be said that the present solid electrolyte material has a sufficient relative density.

[0055] The above relative density is the percentage obtained by dividing the measured density calculated based on the mass and volume of the solid electrolyte by the theoretical density of the solid electrolyte (measured density value / theoretical density value×100), and can be specifically measured using the method described in the following examples.

[0056] The theoretical density of a solid electrolyte is calculated by taking a weighted average of the theoretical density of the crystal structures that make up the solid electrolyte and the content of the crystal structures. For example, if the solid electrolyte has crystal structure 1 at a content of h% and crystal structure 2 at a content of k%, the theoretical density is calculated as (theoretical density of crystal structure 1 × h + theoretical density of crystal structure 2 × k) / 100.

[0057] The content of each crystal structure can be determined by Rietveld analysis.

[0058] As the constituent elements of the present solid electrolyte 1, there are no special restrictions as long as it contains lithium, tantalum, phosphorus and oxygen. From the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density, it is preferred to contain boron element, and may contain one or more elements Ma selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge.

[0059] The content of lithium element in the present solid electrolyte is preferably 5.0 to 20.0 atomic %, more preferably 9.0 to 15.0 atomic %, from the viewpoint of achieving a solid electrolyte with higher lithium ion conductivity.

[0060] In addition, the content of each element in the present solid electrolyte, for example, as a lithium-containing transition metal oxide such as LiCoO2, is measured using a standard powder sample containing Mn, Co, and Ni in a ratio of 1:1:1 by the absolute intensity quantitative method of Auger Electron Spectroscopy (AES). In addition, it can also be obtained by quantitative analysis known in the past. For example, after adding an acid to the sample for thermal decomposition, the thermal decomposition product can be constant in volume, and a high-frequency inductively coupled plasma (ICP) emission analyzer can be used to obtain the content of each element in the present solid electrolyte.

[0061] The content of the tantalum element in the present solid electrolyte is preferably 10.6 to 16.6 atomic %, more preferably 11.0 to 16.0 atomic %, from the viewpoint of achieving a solid electrolyte with higher lithium ion conductivity.

[0062] The phosphorus content in the present solid electrolyte is preferably 5.3 to 8.3 atomic %, more preferably 5.3 atomic % or more and less than 8.3 atomic %, and even more preferably 5.8 to 8.0 atomic %, from the perspective of achieving a solid electrolyte with higher lithium ion conductivity.

[0063] When the present sintered body contains boron, the content of boron in the present solid electrolyte is preferably 0.1 to 5.0 atomic %, more preferably 0.5 to 3.0 atomic %, from the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density.

[0064] When the present solid electrolyte 1 or 2 contains the above-mentioned element Ma, the content of each element Ma in the present solid electrolyte is preferably 0.1 to 5.0 atomic %, more preferably 0.1 to 3.0 atomic %, from the perspective of being able to lower the sintering temperature when producing a solid electrolyte with sufficient ion conductivity and relative density.

[0065] The total ion conductivity of the present solid electrolyte is preferably 2.00×10 -4 S cm -1 More than 3.00×10 -4 S cm -1 above.

[0066] If the total ion conductivity is within the above range, it can be said that the present solid electrolyte has sufficient ion conductivity.

[0067] The total ion conductivity can be specifically measured by the method described in the following examples.

[0068] <Method for producing the present solid electrolyte>

[0069] The present solid electrolyte can be produced, for example, by a method comprising the step A of sintering a component (Z) containing lithium, tantalum, phosphorus, and oxygen as constituent elements. Component (Z) preferably contains boron and may contain the element Ma.

[0070] The sintering temperature in the step A is preferably 500 to 900°C, more preferably 600 to 900°C, and even more preferably 650 to 900°C.

[0071] Even when fired at such a low temperature, a solid electrolyte having sufficient ion conductivity and relative density can be obtained.

[0072] The firing time in the above-mentioned step A varies depending on the firing temperature, but is preferably 12 to 144 hours, and more preferably 48 to 96 hours.

[0073] When the calcination time is within the above range, a solid electrolyte having sufficient ion conductivity and relative density can be obtained even when calcination is performed at a low temperature.

[0074] The calcination in the above-mentioned step A may be performed in the air, but is preferably performed in an atmosphere of nitrogen and / or argon with the oxygen content adjusted to a range of 0 to 20% by volume.

[0075] Alternatively, the calcination in step A may be performed under a reducing gas atmosphere such as a nitrogen-hydrogen mixed gas containing a reducing gas such as hydrogen. The ratio of hydrogen contained in the nitrogen-hydrogen mixed gas may be, for example, 1 to 10% by volume. In addition to hydrogen, ammonia, carbon monoxide, and the like may also be used as the reducing gas.

[0076] In the above-mentioned step A, from the perspective of being able to easily obtain a solid electrolyte with a higher balance between ion conductivity and relative density, it is preferred to sinter the molded body obtained by molding component (Z), and it is more preferred to sinter the molded body obtained by stamping component (Z).

[0077] The pressure during press molding is not particularly limited, but is preferably 50 to 500 MPa, more preferably 100 to 400 MPa.

[0078] The shape of the molded body is not particularly limited, and is preferably a shape that corresponds to the application of the obtained solid electrolyte.

[0079] From the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density, the component (Z) is preferably manufactured using a method (I) comprising a pulverization step of pulverizing (pulverizing and mixing) a pulverization object containing lithium, tantalum, boron, phosphorus and oxygen as constituent elements.

[0080] The shape and size of the component (Z) are not particularly limited, but it is preferably in a particulate (powdered) form, and the average particle size (D50) is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm.

[0081] When D50 of the component (Z) is within the above range, the present solid electrolyte obtained by calcining the component tends to have higher ion conductivity and relative density.

[0082] The pulverization step is preferably performed so that the obtained component (Z) becomes amorphous by a mechanochemical reaction and / or the D50 of the component falls within the above range.

[0083] As the above-mentioned pulverization step, for example, there can be mentioned a method of pulverizing using a roller mill, a ball mill, a small-diameter ball mill (bead mill), a medium stirring mill, a jet mill, a mortar, an automatic mixing mortar, a tank disintegrator, a jet mill, etc. Among them, from the perspective of being able to easily obtain the present solid electrolyte having higher ion conductivity and relative density, the method of pulverizing using a ball mill or a bead mill is preferred, and the method of pulverizing using a ball mill with balls having a diameter of 0.1 to 10 mm is more preferred.

[0084] The time of the pulverization step is preferably 0.5 to 48 hours, more preferably 2 to 48 hours, from the viewpoint of easily obtaining the component (Z) that becomes amorphous by a mechanochemical reaction and / or has a D50 within the above range.

[0085] In the pulverization step, the pulverization and mixing may be performed while heating as needed, but the pulverization and mixing are usually performed at room temperature.

[0086] The pulverization step may be performed in the atmosphere, but is preferably performed in an atmosphere of nitrogen and / or argon with an oxygen content adjusted to a range of 0 to 20% by volume.

[0087] From the viewpoint of easy handling, the raw material used for the material to be pulverized is preferably an inorganic compound.

[0088] The raw materials can be produced by conventionally known methods, or commercially available products can be used.

[0089] As the above-mentioned method (I), for example, there can be mentioned:

[0090] Method (i) using a lithium atom-containing compound, a tantalum atom-containing compound, a boron atom-containing compound, or a phosphorus atom-containing compound as the pulverization target material.

[0091] In addition, in method (i), from the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density, a compound containing the above-mentioned element Ma, in particular at least one compound selected from a compound containing a niobium atom, a compound containing a bismuth atom and a compound containing a silicon atom, can be used.

[0092] Examples of lithium-containing compounds include lithium carbonate (Li2CO3), lithium oxide (Li2O), lithium hydroxide (LiOH), lithium acetate (LiCH3COO), and hydrates thereof. Among these, lithium carbonate, lithium hydroxide, and lithium acetate are preferred due to their ease of decomposition and reaction.

[0093] The lithium atom-containing compound may be used alone or in combination of two or more.

[0094] Examples of compounds containing tantalum atoms include tantalum pentoxide (Ta2O5) and tantalum nitrate (Ta(NO3)5). Among these, tantalum pentoxide is preferred from the perspective of cost.

[0095] The tantalum atom-containing compound may be used alone or in combination of two or more.

[0096] Examples of boron atom-containing compounds include LiBO2, LiB3O5, Li2B4O7, Li3B 11 O 18 、Li3BO3、Li3B7O 12 、Li4B2O5、Li6B4O9、Li 3-x5 B 1-x5 C x5 O3(0<x5<1), Li 4-x6 B 2-x6 C x6O5(0<x6<2), Li 2.4 Al 0.2 BO3, Li 2.7 Al 0.1 BO3, B2O3, H3BO3.

[0097] The boron atom-containing compound may be used alone or in combination of two or more.

[0098] As the compound containing a phosphorus atom, phosphate is preferable. As the phosphate, from the viewpoint of easy decomposition and reaction, for example, diammonium hydrogen phosphate ((NH 4 ) 2 HPO 4 ) and monoammonium dihydrogen phosphate (NH 4 H 2 PO 4 ) can be mentioned.

[0099] The phosphorus atom-containing compound may be used alone or in combination of two or more.

[0100] When the component (Z) contains the element Ma, examples of the compound containing the element Ma include oxides and nitrates.

[0101] Examples of the niobium atom-containing compound in this specification include Nb2O5, LiNbO3, LiNb3O8, and NbPO5.

[0102] The niobium atom-containing compound may be used alone or in combination of two or more.

[0103] Examples of the bismuth atom-containing compounds in this specification include LiBiO2, Li3BiO3, Li4Bi2O5, Li 2.4 Al 0.2 BiO3, Bi2O3.

[0104] The bismuth atom-containing compound may be used alone or in combination of two or more.

[0105] When using a compound containing the element Ma, one type of compound containing the element Ma may be used, or two or more types may be used.

[0106] When Ma is Nb, examples of the compound containing a niobium atom include Nb2O5, LiNbO3, LiNb3O8, and NbPO5.

[0107] The niobium atom-containing compound may be used alone or in combination of two or more.

[0108] When Ma is Bi, examples of compounds containing bismuth atoms include LiBiO2, Li3BiO3, Li4Bi2O5, Li 2.4 Al 0.2 BiO3, Bi2O3.

[0109] The bismuth atom-containing compound may be used alone or in combination of two or more.

[0110] When Ma is Ga or Sn, examples of the oxide include gallium oxide (Ga 2 O 3 ), tin oxide (SnO 2 ), and the like.

[0111] When Ma is Zr, Hf, W or Mo, examples of the oxides include zirconium oxide (ZrO2), hafnium oxide (HfO2), tungsten oxide (WO3), molybdenum oxide (MoO3), etc. When M1 is Zr, Hf, W or Mo, in addition to the oxides, zirconium hydroxide (Zr(OH)4), hafnium hydroxide (Hf(OH)4), tungstic acid (H2WO4), and molybdic acid (H2MoO4) can also be used from the perspective of easy reaction.

[0112] When Ma is Si, examples of the compound containing a silicon atom include SiO2, Li2SiO3, Li2Si2O5, Li2Si3O7, Li4SiO4, Li6Si2O7, and Li8SiO6.

[0113] The silicon atom-containing compound may be used alone or in combination of two or more.

[0114] When Ma is Ge or Al, examples of the oxide include germanium oxide (GeO 2 ), aluminum oxide (Al 2 O 3 ), and the like.

[0115] Examples of the silicon atom-containing compound in this specification include SiO2, Li2SiO3, Li2Si2O5, Li2Si3O7, Li4SiO4, Li6Si2O7, and Li8SiO6.

[0116] The silicon atom-containing compound may be used alone or in combination of two or more.

[0117] The raw materials may be mixed in such a ratio that the content of each constituent element in the obtained solid electrolyte falls within the above range, or such an amount that the obtained solid electrolyte satisfies the stoichiometric formula of the above requirement (II) or (III).

[0118] In addition, during the calcination in the step (A), since lithium atoms are likely to flow out of the system, the lithium atom-containing compound may be used in an excess of about 10% to 20%.

[0119] In the method (i), the raw materials may be mixed before the pulverization step, but preferably, the raw materials are mixed while being pulverized in the pulverization step (pulverization and mixing).

[0120] As the above-mentioned method (I), for example, the following can be adopted:

[0121] Method (ii) using a compound (a) containing lithium, tantalum, phosphorus and oxygen as constituent elements and a boron compound (b) (hereinafter also referred to as compound (b)) as the pulverization target material, or

[0122] Method (iii) using a compound (c) containing lithium, tantalum, boron, phosphorus, and oxygen as constituent elements as the material to be pulverized.

[0123] In addition, in methods (ii) and (iii), from the perspective of being able to lower the sintering temperature when obtaining a solid electrolyte with sufficient ion conductivity and relative density, a compound containing the above-mentioned element Ma, in particular at least one compound selected from a compound containing a niobium atom, a compound containing a bismuth atom, and a compound containing a silicon atom, can be further used.

[0124] In method (ii), compound (a) and compound (b) may be mixed before the pulverization step, but preferably, compound (a) and compound (b) are mixed while being pulverized (pulverization mixing) in the pulverization step.

[0125] Compound (a)

[0126] The compound (a) is a compound containing lithium, tantalum, phosphorus, and oxygen as constituent elements, and is preferably an oxide containing these elements, and more preferably a lithium ion conductive compound containing these elements.

[0127] The compound (a) used in the method (ii) may be one kind or two or more kinds.

[0128] Compound (a) is preferably a compound having a monoclinic crystal structure. Whether compound (a) has a monoclinic crystal structure can be determined, for example, by performing Rietveld analysis on the X-ray diffraction (XRD) pattern of compound (a), specifically by the method described in the following examples.

[0129] Specific examples of compound (a) include compounds (a1) containing lithium, tantalum, phosphorus, and oxygen as constituent elements and further containing one or more elements M1 selected from Bi, Nb, Zr, Ga, Sn, Hf, W, and Mo; and compounds (a2) containing lithium, tantalum, phosphorus, and oxygen as constituent elements and further containing one or more elements M2 selected from Si, Al, and Ge. Among these, compounds (a) whose constituent elements consist solely of lithium, tantalum, phosphorus, and oxygen are preferred, with LiTa2PO8 being more preferred, in order to further enhance the effects of the present invention.

[0130] The compound (a1) is preferably LiTa2PO8, or a compound in which a portion of Ta in LiTa2PO8 is replaced by an element M1, and preferably has a monoclinic structure.

[0131] Specifically, the compound (a1) is preferably composed of the formula Li 1+(5-a)g 〕Ta 2-g M1 g A compound represented by PO8 [M1 is one or more elements M1 selected from Bi, Nb, Zr, Ga, Sn, Hf, W and Mo, 0≤g<1.0, a is the average valence of M1].

[0132] In the present solid electrolyte obtained using compound (a), from the perspective of improving lithium ion conductivity at grain boundaries, M1 is more preferably Nb, Bi, W, or Mo, further preferably Nb, Bi, or W, and particularly preferably Nb.

[0133] The above-mentioned g is preferably 0.95 or less, more preferably 0.90 or less, further preferably 0.85 or less, more preferably 0.80 or less, and particularly preferably 0.75 or less.

[0134] When g is within the above range, the lithium ion conductivity at the grain boundaries of the present solid electrolyte obtained using the compound (a) tends to be improved.

[0135] According to the valence and content of M1, the amount of Li varies corresponding to the average valence of M1 to obtain the charge neutrality of the above-mentioned compound (a). The average valence represented by the above-mentioned a can be calculated as follows. In the case where M1 is composed of two or more elements, the above-mentioned a is calculated by taking a weighted average using the valence of each element and the content of each element. For example, in the case where M1 is composed of 80 atomic % Nb and 20 atomic % Zr, a is calculated as (+5×0.8)+(+4×0.2)=+4.8. In addition, in the case where M1 is composed of 80 atomic % Nb and 20 atomic % W, a is calculated as (+5×0.8)+(+6×0.2)=+5.2.

[0136] The compound (a2) is preferably LiTa2PO8, or a compound in which a portion of P in LiTa2PO8 is replaced by an element M2, and preferably has a monoclinic structure.

[0137] Specifically, the compound (a2) is preferably composed of the formula Li 1+(5-b)k 〕Ta2P 1-k M2 k A compound represented by O8 [M2 is one or more elements M2 selected from Si, Al and Ge, 0≤k<0.7, b is the average valence of M2].

[0138] In the present solid electrolyte obtained using compound (a), M2 is more preferably Si or Al, and even more preferably Si, from the viewpoint of improving lithium ion conductivity at the grain boundaries.

[0139] The above-mentioned k is preferably 0.65 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.

[0140] When k is within the above range, in the solid electrolyte obtained using the compound (a), the total conductivity, which is the sum of the lithium ion conductivity within the crystal grains and at the grain boundaries, tends to be improved.

[0141] The average price represented by b can be calculated in the same way as the average price a.

[0142] The method for producing compound (a) is not particularly limited, and conventionally known production methods such as solid phase reaction and liquid phase reaction can be employed. Specific examples of such production methods include methods comprising at least one mixing step and one calcination step.

[0143] As a mixing step in the method for producing the above-mentioned compound (a), for example, there can be mentioned a step of mixing a lithium atom-containing compound (for example, oxide, carbonate), a tantalum atom-containing compound (for example, oxide, nitrate), a phosphorus atom-containing compound (for example, ammonium salt), and a compound containing element M1 (for example, oxide) and / or a compound containing element M2 (for example, oxide) used as needed as raw materials.

[0144] The above raw materials may be used alone or in combination of two or more.

[0145] Examples of the method for mixing the raw materials include a method using a roll mill, a ball mill, a small-diameter ball mill (bead mill), a media stirring mill, a jet mill, a mortar, an automatic mixing mortar, a tank disintegrator, a jet mill, and the like.

[0146] The mixing ratio of the raw materials may be, for example, a stoichiometric ratio that can provide a desired composition of the compound (a).

[0147] In addition, in the calcination step described later, since lithium atoms are easily released from the system, the lithium-containing compound can be used in an excess of about 10% to 20%. In addition, in the calcination step described later, in order to suppress the formation of by-products, the phosphorus-containing compound can be used in an excess of about 0.1% to 10%.

[0148] During the mixing, the mixing may be performed while heating as necessary, but is usually performed at room temperature.

[0149] The mixing may be performed in the air, but is preferably performed in an atmosphere of nitrogen and / or argon with the oxygen content adjusted to a range of 0 to 20% by volume.

[0150] In the calcination process of the manufacturing method of the above-mentioned compound (a), the mixture obtained in the mixing process is calcined. In the case of performing multiple calcination processes, in order to crush or reduce the particle size of the burned product obtained in the calcination process, a pulverization process using a ball mill or mortar can be provided. In particular, the reaction rate of the phase generation of compound (a) is slow, so sometimes a reaction intermediate is present in the first calcination. In this case, it is preferred to perform the first calcination and then perform the calcination process after performing the pulverization process.

[0151] The calcination step may be performed in the air, but is preferably performed in an atmosphere of nitrogen and / or argon with the oxygen content adjusted to a range of 0 to 20% by volume.

[0152] The firing temperature varies depending on the firing time, but is preferably 800 to 1200°C, more preferably 950 to 1100°C, and even more preferably 950 to 1000°C.

[0153] When the calcination temperature is within the above range, lithium atoms are less likely to flow out of the system, and a compound (a) having high ion conductivity tends to be easily obtained.

[0154] The firing time (the total firing time when the firing steps are performed several times) varies depending on the firing temperature, but is preferably 1 to 16 hours, more preferably 3 to 12 hours.

[0155] When the calcination time is within the above range, lithium atoms are less likely to flow out of the system, and a compound having high ion conductivity tends to be easily obtained.

[0156] The fired product obtained after the firing step may absorb moisture or react with carbon dioxide to deteriorate if left in the air. Therefore, the fired product obtained after the firing step is preferably transferred to a dehumidified inert gas atmosphere for storage when the temperature reaches 200°C or lower during the cooling process after the firing step.

[0157] Boron compounds (b)

[0158] The boron compound (b) is a compound different from the compound (a).

[0159] The compound (b) used in the method (ii) may be one kind or two or more kinds.

[0160] From the viewpoint of easy handling, the compound (b) is preferably an inorganic compound, more preferably a compound containing lithium or hydrogen as a constituent element, and still more preferably a composite oxide containing lithium as a constituent element.

[0161] The compound (b) can be produced by a conventionally known method, or a commercially available product can be used.

[0162] Compound (b) is preferably a crystalline compound. Whether compound (b) is a crystalline compound can be determined based on, for example, the X-ray diffraction (XRD) pattern of compound (b).

[0163] Examples of boron compounds include LiBO2, LiB3O5, Li2B4O7, Li3B 11 O 18 、Li3BO3、Li3B7O 12 、Li4B2O5、Li6B4O9、Li 3-x5 B 1-x5 C x5 O3(0<x5<1), Li 4-x6 B 2-x6 C x6 O5(0<x6<2), Li 2.4 Al 0.2 BO3, Li 2.7 Al 0.1 BO3, B2O3, H3BO3.

[0164] In method (ii), it is preferred to use compound (a) and compound (b) in such an amount that the content of each constituent element in the obtained solid electrolyte falls within the above range, or in such an amount that the obtained solid electrolyte satisfies the stoichiometric formula of the above requirement (II) or (III).

[0165] Compound (c)

[0166] The compound (c) is a compound containing lithium, tantalum, boron, phosphorus, and oxygen as constituent elements, and is preferably an oxide containing these elements, and more preferably a lithium ion conductive compound containing these elements.

[0167] In addition, the compound (c) may contain the above-mentioned element Ma.

[0168] Compound (c) is preferably a compound having a monoclinic crystal structure. Whether compound (c) has a monoclinic crystal structure can be determined, for example, by performing Rietveld analysis on the X-ray diffraction (XRD) pattern of compound (c), specifically by the method described in the following examples.

[0169] The method for producing compound (c) is not particularly limited, and conventionally known production methods such as solid phase reaction and liquid phase reaction can be employed. Specific examples of such production methods include methods comprising at least one mixing step and one calcination step, respectively.

[0170] The mixing step in the method for producing the compound (c) may include, for example, a step of mixing raw materials comprising a lithium atom-containing compound (e.g., oxide, hydroxide, carbonate, acetate), a tantalum atom-containing compound (e.g., oxide, nitrate), a boron atom-containing compound (e.g., oxide), a phosphorus atom-containing compound (e.g., ammonium salt), and, if necessary, a compound containing the metal Ma (e.g., oxide, nitrate). The compound (b) may be used as the boron atom-containing compound.

[0171] The above raw materials may be used alone or in combination of two or more.

[0172] The raw materials may be mixed in such a ratio that the content of each constituent element in the obtained solid electrolyte falls within the above range, or such an amount that the obtained solid electrolyte satisfies the stoichiometric formula of the above requirement (II) or (III).

[0173] In addition, during the calcination in step (A), since lithium atoms tend to flow out of the system, the lithium-containing compound may be used in an excess of about 10% to 20%. In addition, in the calcination step described later, in order to suppress the formation of by-products, the phosphorus-containing compound may be used in an excess of about 0.1% to 10%.

[0174] Examples of the method for mixing the raw materials and the conditions for mixing (temperature, atmosphere, etc.) include the same methods and conditions as those in the mixing step for producing the compound (a).

[0175] In the calcining step of the method for producing compound (c), the mixture obtained in the mixing step is calcined. When the calcining step is performed multiple times, a pulverizing step using a ball mill or mortar can be provided to crush or reduce the particle size of the calcined product obtained in the calcining step. However, unlike the production of compound (a), the reaction rate of phase formation of compound (c) is high, and the desired compound (c) can be produced in a single calcining step. Therefore, it is preferred to produce compound (c) in a single calcining step.

[0176] As the conditions (temperature, time, atmosphere, etc.) in the above-mentioned calcination step, for example, the same conditions as those in the calcination step when producing the above-mentioned compound (a) can be cited. In addition, based on the same reasons as when producing compound (a), the calcined product obtained after the calcination step is preferably transferred to a dehumidified inert gas atmosphere for storage, similarly to when producing compound (a).

[0177] All-Solid-State Battery

[0178] An all-solid-state battery (hereinafter also referred to as "this battery") involved in one embodiment of the present invention includes a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, and a solid electrolyte layer located between the positive electrode and the negative electrode, wherein the solid electrolyte layer includes this solid electrolyte.

[0179] The present battery may be a primary battery or a secondary battery, but is preferably a secondary battery, more preferably a lithium ion secondary battery, from the viewpoint of further exerting the effects of the present invention.

[0180] The structure of the present battery is not particularly limited as long as it includes a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive and negative electrodes, and may be any of so-called thin film type, laminated type, and bulk type.

[0181] Solid electrolyte layer

[0182] The solid electrolyte layer is not particularly limited as long as it contains the present solid electrolyte, and may contain conventionally known additives used in solid electrolyte layers of all-solid-state batteries as needed, but is preferably composed of the present solid electrolyte.

[0183] The thickness of the solid electrolyte layer can be appropriately selected depending on the structure of the battery to be formed (thin film type, etc.), and is preferably 50 nm to 1000 μm, and more preferably 100 nm to 100 μm.

[0184] <Positive electrode>

[0185] The positive electrode is not particularly limited as long as it contains a positive electrode active material, but preferably, a positive electrode containing a positive electrode current collector and a positive electrode active material layer is used.

[0186] [Positive Electrode Active Material Layer]

[0187] The positive electrode active material layer is not particularly limited as long as it contains a positive electrode active material, but preferably contains a positive electrode active material and a solid electrolyte, and may further contain additives such as a conductive aid and a sintering aid.

[0188] The thickness of the positive electrode active material layer can be appropriately selected depending on the structure of the battery to be formed (thin film type, etc.), and is preferably 10 to 200 μm, more preferably 30 to 150 μm, and even more preferably 50 to 100 μm.

[0189] Positive electrode active material

[0190] Examples of positive electrode active materials include LiCo oxide, LiNiCo oxide, LiNiCoMn oxide, LiNiMn oxide, LiMn oxide, LiMn spinel, LiMnNi oxide, LiMnAl oxide, LiMnMg oxide, LiMnCo oxide, LiMnFe oxide, LiMnZn oxide, LiCrNiMn oxide, LiCrMn oxide, lithium titanate, lithium metal phosphate, transition metal oxides, titanium sulfide, graphite, hard carbon, lithium nitride containing transition metals, silicon oxide, lithium silicate, lithium metal, lithium alloy, solid solution containing Li, and lithium storage intermetallic compound.

[0191] Among them, LiNiCoMn oxide, LiNiCo oxide, and LiCo oxide are preferred, and LiNiCoMn oxide is more preferred, from the perspectives of good affinity with solid electrolytes, excellent balance among macroscopic conductivity, microscopic conductivity, and ionic conductivity, high average potential, and the ability to improve energy density or battery capacity in a balance between specific capacity and stability.

[0192] Alternatively, the positive electrode active material may be surface-coated with an ion-conductive oxide such as lithium niobate, lithium phosphate, or lithium borate.

[0193] The positive electrode active material used in the positive electrode active material layer may be one kind or two or more kinds.

[0194] Preferred examples of the positive electrode active material include LiM3PO4 [M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements of V and O], LiM5VO4 [M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti], Li2M6P2O7 [M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements of V and O], LiVP2O7, Li x7 V y7 M7 z7 [2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr], Li 1+x8 Al x8 M8 2-x8 (PO4)3[0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge], LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2, LiCoO2, LiNiO2, LiMn2O4, Li2CoP2O7, Li3V2(PO4)3, Li3Fe2(PO4)3, LiNi 0.5 Mn 1.5 O4、Li4Ti5O 12 .

[0195] The positive electrode active material is preferably in a particulate form, and the 50% diameter in the volume-based particle size distribution is preferably 0.1 to 30 μm, more preferably 0.3 to 20 μm, further preferably 0.4 to 10 μm, and particularly preferably 0.5 to 3 μm.

[0196] The positive electrode active material preferably has an aspect ratio, which is the ratio of the major axis to the minor axis (major axis length / minor axis length), of less than 3, more preferably less than 2.

[0197] The positive electrode active material may be formed into secondary particles. In this case, the 50% diameter of the primary particles in the number-based particle size distribution is preferably 0.1 to 20 μm, more preferably 0.3 to 15 μm, further preferably 0.4 to 10 μm, and particularly preferably 0.5 to 2 μm.

[0198] The content of the positive electrode active material in the positive electrode active material layer is preferably 20 to 80 volume %, more preferably 30 to 70 volume %.

[0199] When the content of the positive electrode active material is within the above range, the positive electrode active material functions well, and there is a tendency that a battery with a high energy density can be easily obtained.

[0200] Solid electrolyte

[0201] The solid electrolyte that can be used in the positive electrode active material layer is not particularly limited, and conventionally known solid electrolytes can be used. However, the present solid electrolyte is preferably used from the viewpoint of further exerting the effects of the present invention.

[0202] The solid electrolyte used in the positive electrode active material layer may be one kind or two or more kinds.

[0203] ·additive

[0204] Preferred examples of the conductive additive include metal materials such as Ag, Au, Pd, Pt, Cu, and Sn, and carbon materials such as acetylene black, Ketjen black, carbon nanotubes, and carbon nanofibers.

[0205] As the sintering aid, compounds similar to the compound (b) described above, compounds containing niobium atoms, compounds containing bismuth atoms, and compounds containing silicon atoms are preferred.

[0206] The additives used in the positive electrode active material layer may be one kind or two or more kinds.

[0207] Positive electrode collector

[0208] The positive electrode current collector is not particularly limited as long as its material is a material that conducts electrons without inducing an electrochemical reaction. As the material of the positive electrode current collector, for example, a metal element such as copper, aluminum, iron, an alloy containing these metals, antimony-doped tin oxide (ATO), tin-doped indium oxide (ITO) and other conductive metal oxides can be cited.

[0209] Alternatively, a positive electrode current collector may be one having a conductive adhesive layer provided on its surface. Examples of the conductive adhesive layer include a layer containing a granular conductive material or a fibrous conductive material.

[0210] Negative electrode

[0211] The negative electrode is not particularly limited as long as it contains a negative electrode active material, but preferably, a negative electrode containing a negative electrode current collector and a negative electrode active material layer is used.

[0212] [Negative Electrode Active Material Layer]

[0213] The negative electrode active material layer is not particularly limited as long as it contains a negative electrode active material, but preferably contains a negative electrode active material and a solid electrolyte, and may further contain additives such as a conductive aid and a sintering aid.

[0214] The thickness of the negative electrode active material layer can be appropriately selected depending on the structure of the battery to be formed (thin film type, etc.), and is preferably 10 to 200 μm, more preferably 30 to 150 μm, and even more preferably 50 to 100 μm.

[0215] Negative electrode active material

[0216] Examples of the negative electrode active material include lithium alloys, metal oxides, graphite, hard carbon, soft carbon, silicon, silicon alloys, silicon oxide SiO n (0<n≤2), silicon / carbon composite material, composite material containing silicon domains in the pores of porous carbon, lithium titanate, and graphite coated with lithium titanate.

[0217] Among them, silicon / carbon composite materials and composite materials containing silicon domains in the pores of porous carbon have high specific capacity and can improve energy density and battery capacity, so they are preferred. More preferably, composite materials containing silicon domains in the pores of porous carbon have excellent slackness in the volume expansion of silicon accompanying lithium absorption / release, and can well maintain the balance of macroscopic conductivity, microscopic conductivity and ion conductivity. Particularly preferably, the silicon domain is amorphous, the size of the silicon domain is less than 10nm, there are pores from porous carbon near the silicon domain, and a composite material containing silicon domains in the pores of porous carbon.

[0218] Preferred examples of the negative electrode active material include LiM3PO4 [M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements of V and O], LiM5VO4 [M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti], Li2M6P2O7 [M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements of V and O], LiVP2O7, Li x7 V y7 M7 z7 [2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr], Li 1+x8 Al x8 M8 2-x8 (PO4)3[0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge], (Li 3-a9x9+(5-b9)y9 M9 x9 )(V 1-y9 M10 y9 )O4[M9 is one or more elements selected from Mg, Al, Ga and Zn, M10 is one or more elements selected from Zn, Al, Ga, Si, Ge, P and Ti, 0≤x9≤1.0, 0≤y9≤0.6, a9 is the average valence of M9, b9 is the average valence of M10], LiNb2O7, Li4Ti5O 12 、Li4Ti5PO 12 , TiO2, LiSi, graphite.

[0219] The negative electrode active material is preferably in particulate form, and the 50% diameter in its volume-based particle size distribution, aspect ratio, and the 50% diameter in its number-based particle size distribution of primary particles when the negative electrode active material forms secondary particles are preferably within the same ranges as those of the positive electrode active material.

[0220] The content of the negative electrode active material in the negative electrode active material layer is preferably 20 to 80% by volume, more preferably 30 to 70% by volume.

[0221] When the content of the negative electrode active material is within the above range, the negative electrode active material functions well, and there is a tendency that a battery with a high energy density can be easily obtained.

[0222] Solid electrolyte

[0223] The solid electrolyte that can be used in the negative electrode active material layer is not particularly limited, and conventionally known solid electrolytes can be used. However, the present solid electrolyte is preferably used from the viewpoint of further exerting the effects of the present invention.

[0224] The solid electrolyte used in the negative electrode active material layer may be one kind or two or more kinds.

[0225] ·additive

[0226] Preferred examples of the conductive additive include metal materials such as Ag, Au, Pd, Pt, Cu, and Sn, and carbon materials such as acetylene black, Ketjen black, carbon nanotubes, and carbon nanofibers.

[0227] As the sintering aid, compounds similar to the compound (b) described above, compounds containing niobium atoms, compounds containing bismuth atoms, and compounds containing silicon atoms are preferred.

[0228] The additives used in the negative electrode active material layer may be one kind or two or more kinds.

[0229] Negative electrode collector

[0230] As the negative electrode current collector, the same current collector as the positive electrode current collector can be used.

[0231] <Method for manufacturing all-solid-state batteries>

[0232] All-solid-state batteries can be formed, for example, by a known powder molding method. For example, a positive electrode current collector, a positive electrode active material layer powder, a solid electrolyte layer powder, a negative electrode active material layer powder, and a negative electrode current collector are sequentially stacked and powder molded simultaneously, thereby simultaneously forming the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer, and connecting the positive electrode current collector, the positive electrode active material layer, the solid electrolyte layer, the negative electrode active material layer, and the negative electrode current collector.

[0233] When the powder is molded, it is preferred to sinter it at the same temperature as that in the step A while applying a pressure substantially equivalent to that in the press molding.

[0234] According to one embodiment of the present invention, even if the firing temperature during the production of the all-solid-state battery is low, an all-solid-state battery with sufficient ion conductivity can be obtained, thereby suppressing the decomposition or deterioration of other materials such as the positive electrode or negative electrode materials, and producing the all-solid-state battery in an economical and equipment-saving manner.

[0235] Alternatively, the positive electrode active material layer, solid electrolyte layer, and negative electrode active material layer may be individually subjected to the above-described powder molding. When using the obtained layers to produce an all-solid-state battery, each layer is preferably pressed and fired.

[0236] In addition, an all-solid-state battery can also be produced by the following method, for example.

[0237] A paste for forming each layer is prepared by appropriately mixing a solvent, resin, etc. with the material for forming the positive electrode active material layer, the material for forming the solid electrolyte layer, and the material for forming the negative electrode active material layer. This paste is then applied to a substrate and dried to produce green sheets for the positive electrode active material layer, solid electrolyte layer, and negative electrode active material layer. Next, the substrate is peeled from each green sheet, and the positive electrode active material layer, solid electrolyte layer, and negative electrode active material layer green sheets are stacked in sequence. After being thermocompressed at a predetermined pressure, the stack is sealed in a container and pressurized by methods such as hot isostatic pressing, cold isostatic pressing, and hydrostatic pressing to produce a laminated structure.

[0238] Then, if necessary, the stacked structure is subjected to a degreasing treatment at a predetermined temperature and then to a sintering treatment to produce a stacked sintered body.

[0239] The firing temperature in this firing treatment is preferably the same temperature as the firing temperature in the above-mentioned step A.

[0240] Next, as necessary, a positive electrode current collector and a negative electrode current collector may be formed on both main surfaces of the stacked sintered body by sputtering, vacuum deposition, coating or dipping of a metal paste, etc., thereby producing an all-solid-state battery.

[0241] Example

[0242] Hereinafter, the present invention will be described in detail based on Examples. However, the present invention is not limited to these Examples.

[0243] [Synthesis Example 1] Synthesis of Li4B2O5

[0244] Lithium hydroxide monohydrate (LiOH·H2O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 98.0% or higher) and boric acid (H3BO3) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.5% or higher) were weighed so that the atomic ratio of lithium to boron (Li:B) was 2.00:1.00. The weighed raw material powders were ground and mixed in an agate mortar for 15 minutes to obtain a mixture.

[0245] The obtained mixture was placed in an alumina container and heated to 500°C at a heating rate of 10°C / min in an atmosphere of air (flow rate: 100 mL / min) using a rotary sintering furnace (manufactured by Motoyama Co., Ltd.). The mixture was sintered at 500°C for 2 hours to obtain a primary sintered product.

[0246] The obtained primary fired product was crushed and mixed in an agate mortar for 15 minutes, and the obtained mixture was placed in an alumina container. Using a rotary firing furnace (manufactured by Motoyama Co., Ltd.), the temperature was raised to 630°C at a heating rate of 10°C / min in an atmosphere of air (flow rate: 100 mL / min), and fired at 630°C for 24 hours to obtain a secondary fired product (Li4B2O5).

[0247] The obtained secondary fired product was cooled to room temperature, taken out from the rotary firing furnace, and stored in a dehumidified nitrogen atmosphere.

[0248] [Synthesis Example 2] Synthesis of Li3BO3

[0249] Lithium hydroxide monohydrate (LiOH·H2O) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with a purity of 98.0% or more) and boric acid (H3BO3) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with a purity of 99.5% or more) were weighed so that the atomic ratio of lithium to boron (Li:B) became 3.00:1.00. Except for this, a secondary calcined product (Li3BO3) was obtained in the same manner as in Synthesis Example 1.

[0250] [Example 1]

[0251] An appropriate amount of toluene was added to tantalum pentoxide (Ta2O5) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%), and the mixture was pulverized for 2 hours using a zirconia ball mill (zirconia balls: 3 mm in diameter).

[0252] Next, lithium carbonate (Li2CO3) (manufactured by Sigma-Aldrich, with a purity of 99.0% or greater), the crushed tantalum pentoxide (Ta2O5) described above, the Li4B2O5 ​​obtained in Synthesis Example 1, and diammonium hydrogen phosphate ((NH4)2HPO4) (manufactured by Sigma-Aldrich, with a purity of 98% or greater) were weighed so that the atomic ratio of lithium, tantalum, boron, and phosphorus (Li:Ta:B:P) satisfied the stoichiometric formula shown in Table 1. An appropriate amount of toluene was added to each weighed raw material powder, and the mixture was pulverized and mixed for 2 hours using a zirconia ball mill (zirconia balls: 1 mm diameter) to obtain a mixture.

[0253] The obtained mixture was subjected to a pressure of 40 MPa using a tablet molding machine and a hydraulic press to form a disc-shaped molded body with a diameter of 10 mm and a thickness of 1 mm. The disc-shaped molded body was then subjected to a pressure of 300 MPa by CIP (cold isostatic pressing) to produce granules.

[0254] The obtained particles were placed in an alumina container and heated to 850°C at a heating rate of 10°C / min in an air atmosphere (flow rate: 100 mL / min) using a rotary sintering furnace (manufactured by Motoyama Co., Ltd.). The mixture was sintered at this temperature for 96 hours to obtain a sintered body.

[0255] The obtained fired product was cooled to room temperature, taken out from the rotary firing furnace, and stored in a dehumidified nitrogen atmosphere to obtain a solid electrolyte.

[0256] [Examples 2 to 4]

[0257] A solid electrolyte was produced in the same manner as in Example 1 except that the mixing ratio of the raw materials was changed so that the atomic ratio of lithium, tantalum, boron, and phosphorus satisfied the stoichiometric formula in Table 1.

[0258] [Example 5]

[0259] A solid electrolyte was produced in the same manner as in Example 1 except that Li3BO3 obtained in Synthesis Example 2 was used instead of Li4B2O5 ​​and that the raw material powders were used so that the atomic ratios of lithium, tantalum, boron and phosphorus satisfied the stoichiometric formula in Table 1.

[0260] [Example 6]

[0261] A solid electrolyte was produced in the same manner as in Example 1 except that boric acid (H3BO3) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with a purity of 99.5% or more) was used instead of Li4B2O5, and each raw material powder was used in such a manner that the atomic ratio of lithium, tantalum, boron and phosphorus satisfied the stoichiometric formula in Table 1.

[0262] [Examples 7 and 8]

[0263] An appropriate amount of toluene was added to niobium pentoxide (Nb2O5) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%), and the mixture was pulverized for 2 hours using a zirconia ball mill (zirconia balls: 3 mm in diameter).

[0264] On the basis of Example 1, the above-mentioned crushed niobium pentoxide (Nb2O5) was further used, and the raw material powders were used in a manner such that the atomic ratio of lithium, tantalum, niobium, boron and phosphorus (Li:Ta:Nb:B:P) satisfied the stoichiometric formula of Table 1. Except for this, a solid electrolyte was produced in the same manner as Example 1.

[0265] [Example 9]

[0266] On the basis of Example 1, silicon oxide (SiO2) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with a purity of 99.9%) was further used, and each raw material powder was used in a manner such that the atomic ratio of lithium, tantalum, boron, phosphorus and silicon (Li:Ta:B:P:Si) satisfied the stoichiometric formula in Table 1. Except for this, a solid electrolyte was produced in the same manner as in Example 1.

[0267] [Comparative Example 1]

[0268] Lithium carbonate (Li2CO3) (manufactured by Sigma-Aldrich, purity 99.0% or higher), tantalum pentoxide (Ta2O5) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.9%), and diammonium hydrogen phosphate ((NH4)2HPO4) (manufactured by Sigma-Aldrich, purity 98% or higher) were weighed so that the atomic ratio of lithium, tantalum, and phosphorus (Li:Ta:P) satisfied the stoichiometric formula shown in Table 1. Furthermore, to account for lithium atoms released from the system during the calcination step, lithium carbonate was weighed in an amount equal to 1.1 times the atomic weight of lithium listed in Table 1. Furthermore, to suppress the formation of by-products during the calcination step, diammonium hydrogen phosphate was weighed in an amount equal to 1.065 times the atomic weight of phosphorus listed in Table 1. An appropriate amount of toluene was added to each weighed raw material powder, and the mixture was pulverized and mixed for 2 hours using a zirconia ball mill (zirconia balls: 1 mm diameter) to produce a primary mixture.

[0269] The obtained primary mixture was placed in an alumina container and heated to 1000°C at a heating rate of 10°C / min in an atmosphere of air (flow rate: 100 mL / min) using a rotary sintering furnace (manufactured by Motoyama Co., Ltd.). The mixture was sintered at 1000°C for 4 hours to obtain a primary sintered product.

[0270] The obtained primary fired product was pulverized and mixed in an agate mortar for 15 minutes to obtain a secondary mixture. The obtained secondary mixture was placed in an alumina container and heated to 1000°C at a rate of 10°C / min in a rotary sintering furnace (produced by Motoyama Co., Ltd.) under an atmosphere of air (flow rate: 100 mL / min). The mixture was then sintered at 1000°C for 1 hour to obtain a secondary fired product.

[0271] An appropriate amount of toluene was added to the obtained secondary fired product, and the mixture was pulverized and mixed for 2 hours using a zirconia ball mill (zirconia balls: 1 mm in diameter) to obtain a tertiary mixture.

[0272] The obtained tertiary mixture was subjected to a pressure of 40 MPa using a tablet forming machine and a hydraulic press to form a disc-shaped molded body with a diameter of 10 mm and a thickness of 1 mm. The disc-shaped molded body was then subjected to a pressure of 300 MPa using CIP (cold isostatic pressing) to produce granules.

[0273] The obtained particles were placed in an alumina container and heated to 850°C at a heating rate of 10°C / min in an air atmosphere (flow rate: 100 mL / min) using a rotary sintering furnace (manufactured by Motoyama Co., Ltd.). The mixture was sintered at this temperature for 96 hours to obtain a sintered body.

[0274] The obtained sintered body was cooled to room temperature, taken out from the rotary sintering furnace, and stored in a dehumidified nitrogen atmosphere to obtain a solid electrolyte.

[0275] <Powder X-ray Diffraction (XRD)>

[0276] The obtained solid electrolyte was pulverized in an agate mortar for 30 minutes to obtain a powder for XRD measurement.

[0277] The resulting powder for XRD measurement was subjected to X-ray diffraction measurement using a Panalytical MPD powder X-ray diffractometer (manufactured by Spectris Corporation) (Cu-Kα radiation (output: 45 kV, 40 mA), diffraction angle 2θ range of 10-50°, step width: 0.013°, incident side Sollerslit: 0.04 rad, incident side anti-scatter slit: 2°, receiving side Sollerslit: 0.04 rad, receiving side anti-scatter slit: 5 mm) to obtain an X-ray diffraction (XRD) pattern. The resulting XRD pattern was then subjected to Rietveld analysis using the known analysis software RIETAN-FP (available from the developer Fujio Izumi's website, "RIETAN-FP VENUS System Distribution File" (http: / / fujioizumi.verse.jp / download / download.html)) to confirm the crystal structure and the content of each crystal structure.

[0278] The XRD patterns of the solid electrolytes obtained in Examples 4, 6 and Comparative Example 1 are shown in FIG. Figure 1 .

[0279] according to Figure 1, only the peak derived from the LiTa2PO8 structure was observed in Comparative Example 1. In the solid electrolyte obtained in Example 4, in addition to the peak derived from the LiTa2PO8 structure, a peak derived from LiTa3O8 (ICSD code: 493) and a peak derived from Ta2O5 (ICSD code: 66366) were observed. In the solid electrolyte obtained in Example 6, a peak derived from TaPO5 (ICSD code: 202041) was observed.

[0280] <Relative density>

[0281] The mass of the prepared solid electrolyte was measured using an electronic balance. The volume was then measured using a micrometer based on the actual dimensions of the solid electrolyte. The density (measured value) of the solid electrolyte was calculated by dividing the measured mass by the volume, and the relative density (%) was calculated as the percentage of the measured value relative to the theoretical value (measured density value / theoretical density value × 100). The results are shown in Table 1.

[0282] In addition, the theoretical value of the density of the solid electrolyte is calculated by using the content of each crystal structure obtained by Rietveld analysis, and taking a weighted average of the theoretical density of the crystal structure based on LiTa2PO8 that constitutes the solid electrolyte and the theoretical density of the crystal structures based on LiTa3O8, Ta2O5 and TaPO5.

[0283] Total conductivity

[0284] Gold layers were formed on both surfaces of the obtained solid electrolyte using a sputtering machine to obtain measurement particles for evaluating ion conductivity.

[0285] The obtained test particles were kept in a constant temperature bath at 25°C for 2 hours before measurement. Next, an impedance analyzer (Solartron Analytical, model: 1260A) was used at 25°C to perform AC impedance measurement in the frequency range of 1 Hz to 10 MHz under an amplitude of 25 mV. The equivalent circuit analysis software ZView included with the device was used to fit the obtained impedance spectrum with an equivalent circuit, and the lithium ion conductivity within the grains and at the grain boundaries was calculated. The total conductivity was calculated by summing them. The results are shown in Table 1.

[0286]

[0287] As shown in Table 1, the solid electrolyte having a crystal structure based on LiTa2PO8 and a crystal structure based on at least one compound selected from LiTa3O8, Ta2O5 and TaPO5, and the solid electrolyte having a crystal structure based on the stoichiometric formula Li a1 Ta b1 Bc1 P d1 O e1 [0.5<a1<2.0、1.0<b1≤2.0、0<c1<0.5、0.5<d1<1.0、5.0<e1≤8.0], or a solid electrolyte represented by the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 The solid electrolyte represented by [0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb, Zr, Ga, Sn, Hf, Bi, W, Mo, Si, Al and Ge] has a good balance between relative density and conductivity even if it is a solid electrolyte obtained by sintering at a low temperature.

Claims

1. A lithium ion conductive solid electrolyte having: Based on the crystal structure of LiTa2PO8; and Based on the crystal structure of at least one compound selected from LiTa3O8, Ta2O5 and TaPO5, According to the stoichiometric formula Li a1 Ta b1 B c1 P d1 O e1 express, 0.5<a1<2.0, 1.0<b1≤2.0, 0<c1<0.5, 0.5<d1<1.0, 5.0<e1≤8.

0.

2. The lithium ion conductive solid electrolyte according to claim 1, The content of tantalum element is 10.6 to 16.6 atomic %.

3. The lithium ion conductive solid electrolyte according to claim 1 or 2, The content of phosphorus element is 5.3 to 8.3 atomic %.

4. The lithium ion conductive solid electrolyte according to claim 1 or 2, The content of lithium element is 5.0 to 20.0 atomic %.

5. The lithium ion conductive solid electrolyte according to claim 1 or 2, The relative density, which is a percentage of the actual density calculated from the mass and volume of the lithium ion conductive solid electrolyte relative to the theoretical density of the crystal structure constituting the lithium ion conductive solid electrolyte, is 60% or more.

6. A lithium ion conductive solid electrolyte having: Based on the crystal structure of LiTa2PO8; and Based on the crystal structure of at least one compound selected from LiTa3O8, Ta2O5 and TaPO5, According to the stoichiometric formula Li a2 Ta b2 Ma c2 B d2 P e2 O f2 express, 0.5<a2<2.0, 1.0<b2≤2.0, 0<c2<0.5, 0<d2<0.5, 0.5<e2<1.0, 5.0<f2≤8.0, Ma is one or more elements selected from Nb and Si.

7. The lithium ion conductive solid electrolyte according to claim 6, The content of tantalum element is 10.6 to 16.6 atomic %.

8. The lithium ion conductive solid electrolyte according to claim 6 or 7, The content of phosphorus element is 5.3 to 8.3 atomic %.

9. The lithium ion conductive solid electrolyte according to claim 6 or 7, The content of lithium element is 5.0 to 20.0 atomic %.

10. The lithium ion conductive solid electrolyte according to claim 6 or 7, The relative density, which is a percentage of the actual density calculated from the mass and volume of the lithium ion conductive solid electrolyte relative to the theoretical density of the crystal structure constituting the lithium ion conductive solid electrolyte, is 60% or more.

11. An all-solid-state battery comprising a positive electrode, a negative electrode and a solid electrolyte layer, The positive electrode has a positive electrode active material, The negative electrode has a negative electrode active material, The solid electrolyte layer is located between the positive electrode and the negative electrode, The solid electrolyte layer includes the lithium ion conductive solid electrolyte according to any one of claims 1 to 10.

12. The all-solid-state battery according to claim 11, wherein the positive electrode active material comprises a material selected from the group consisting of LiM3PO4, LiM5VO4, Li2M6P2O7, LiVP2O7, Li x7 V y7 M7 z7 , Li 1+x8 Al x8 M8 2-x8 (PO4)3、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiCoO2, LiNiO2, LiMn2O4, Li2CoP2O7, Li3V2(PO4)3, Li3Fe2(PO4)3, LiNi 0.5 Mn 1.5 O4 and Li4Ti5O 12 One or more compounds of M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements V and O, M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti, M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements V and O, 2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr, 0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge.

13. The all-solid-state battery according to claim 11 or 12, wherein the negative electrode active material comprises a material selected from the group consisting of LiM3PO4, LiM5VO4, Li2M6P2O7, LiVP2O7, Li x7 V y7 M7 z7 , Li 1+x8 Al x8 M8 2-x8 (PO4)3、(Li 3-a9x9+(5-b9)y9 M9 x9 )(V 1- y9 M10 y9 )O4, LiNb2O7, Li4Ti5O 12 、Li4Ti5PO 12 , TiO2, LiSi and graphite, M3 is one or more elements selected from Mn, Co, Ni, Fe, Al, Ti and V, or two elements V and O, M5 is one or more elements selected from Fe, Mn, Co, Ni, Al and Ti, M6 is one or more elements selected from Fe, Mn, Co, Ni, Al, Ti and V, or two elements V and O, 2≤x7≤4, 1≤y7≤3, 0≤z7≤1, 1≤y7+z7≤3, M7 is one or more elements selected from Ti, Ge, Al, Ga and Zr, 0≤x8≤0.8, M8 is one or more elements selected from Ti and Ge, M9 is one or more elements selected from Mg, Al, Ga and Zn, M10 is one or more elements selected from Zn, Al, Ga, Si, Ge, P and Ti, 0≤x9≤1.0, 0≤y9≤0.6, a9 is the average price of M9, and b9 is the average price of M10.

14. The all-solid-state battery according to claim 11 or 12, The positive electrode and the negative electrode contain the lithium ion conductive solid electrolyte according to any one of claims 1 to 10.