A sintered ore containing P2 iron ore powder and a preparation method thereof
By using the combination of P2 iron ore powder and solid fuel, combined with sintering technology, the problem of high sintering ore costs is solved, cost reduction and yield improvement are achieved, and sintering performance is improved.
Patent Information
- Application Number
- CN202211302839.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-10-24
AI Technical Summary
The high production cost of sintered ore is limited by the scarcity and high-quality iron ore powder, which leads to a severe situation in the steel market, and it is necessary to find low-priced alternative materials to reduce costs.
The low-priced P2 iron ore powder is used to combine with Jinbuba powder, Tok powder, Indian powder, WPF powder, Newman powder, Mike powder, and stone powder, and add back ore and solid fuel to prepare sintered ore through sintering technology and adjust raw materials Composition and sintering conditions to improve yield and utilization coefficient.
While ensuring the quality of the production, the cost of sintered ore is reduced, the sintering yield and utilization coefficient are improved, and the vertical sintering speed and reduction performance are improved through crystallization water in P2 ore powder.
Smart Images

Figure BDA0003905503550000041 
Figure BDA0003905503550000051 
Figure BDA0003905503550000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sintering ore, and in particular to a sintered ore containing P2 iron ore powder and a preparation method thereof. Background Art
[0002] Sintering is the process of mixing and pelletizing various iron-containing powdered raw materials, and then subjecting the materials to a series of physical and chemical changes on sintering equipment to bond the ore powder particles into blocks. Sintering is the main raw material for blast furnace ironmaking. Not only does its quality have an important impact on the blast furnace smelting process, but its production cost also directly affects the comprehensive cost of the ironmaking process.
[0003] However, affected by mineral resources and market environment, high-quality iron ore powder is becoming less and less, and the price is expensive, which makes the steel market situation severe and increases the composition of sintered ore. Therefore, it is necessary to use low-priced iron ore powder and further expand the scope of use of external powder to reduce the cost of sintered ore. P2 iron ore powder is cheap, but there is no report on the application of P2 iron ore powder in sintered ore. Summary of the invention
[0004] The present invention provides a sintered ore containing P2 iron ore powder and a preparation method thereof, which solves the problem of high production cost of sintered ore in the related art.
[0005] The technical solution of the present invention is as follows:
[0006] A sintered ore containing P2 iron ore powder, comprising the following components: mixed ore powder, return ore, flux, and solid fuel;
[0007] The mixed ore powder includes the following components: P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, Mike powder, stone powder;
[0008] The solid fuel includes washed coal and coking coal.
[0009] As a further technical solution, the mixed mineral powder includes the following components by weight percentage: 25-35% P2 iron ore powder, 10-18% Jinbuba powder, 13-16% Tok powder, 10% India powder, 10-15% WPF powder, 10% Newman powder, 9-12% Mike powder, and 2-4% stone powder.
[0010] As a further technical solution, the mixed mineral powder includes the following components by weight percentage: 25% P2 iron ore powder, 13% Jinbuba powder, 16% Tok powder, 10% India powder, 10% WPF powder, 10% Newman powder, 12% Mike powder, and 4% stone powder.
[0011] As a further technical solution, the amount of the returned ore added is 20-23.7% of the total weight of all raw materials.
[0012] As a further technical solution, the amount of solid fuel added is 5.5% of the total weight of all raw materials.
[0013] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0014] S1, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel, and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture;
[0015] S2. Sintering the mixed material to obtain sintered ore.
[0016] As a further technical solution, during the sintering process in step S2, the negative pressure of the flue is 13.2-14.6 KPa, and the exhaust gas temperature is 115-125°C.
[0017] As a further technical solution, in step S1, 7.5-8.5% of the total weight of the mixture and water is added during the mixing process, wherein 80% of the total water is added in the first mixing and the remaining water is added in the second mixing.
[0018] As a further technical solution, the main chemical composition of the P2 iron ore powder is TFe 57.34%, SiO2 6.34%, CaO 0.13%, Al2O3 3.33%, MgO 0.08%, TiO2 0.16%, P2O5 0.062%, S 0.034%, FeO 4.59%, LOI 10.7%, and H2O 9.98%.
[0019] As a further technical solution, the particle size composition of the P2 iron ore powder is 5.3% 10mm, 6.4% 8mm, 12.3% 5mm, 11.5% 3mm, 3.4% 2mm, 20.2% 1mm, 14.4% 0.5mm, 12.7% 0.25mm, 5.2% 0.125mm, 6.8% 0.063mm, and 1.8% -0.063mm.
[0020] The working principle and beneficial effects of the present invention are:
[0021] 1. The present invention adopts low-priced P2 iron ore powder and Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, Mike powder, stone powder, and adds return ore and solid fuel to sinter to obtain sintered ore, which reduces the production cost. The stone powder with complementary microscopic characteristics is selected for use. Under the premise of ensuring the quality of sintered ore, the proportion of stone powder is increased from 2% to 4%, reducing the cost of sintered ore. In addition, P2 ore powder contains a certain amount of crystal water, which can increase the vertical sintering speed and improve the reduction performance of sintered ore.
[0022] 2. The present invention finds that when the proportion of P2 iron ore powder is 25%, the proportion of 5-10 mm particle size in the sintered ore is small. By adjusting the proportion of P2 iron ore powder in the raw materials and adjusting the composition of other raw materials according to the particle size composition of P2, the reduction performance of the sintered ore is improved, the vertical sintering speed is increased, and the sintering yield and utilization coefficient are improved. Increasing or decreasing the proportion of P2 iron ore powder will reduce the reduction performance of the sintered ore, the sintering yield and utilization coefficient. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The solid fuels in Examples 1-5 of the present invention are all mixtures of clean coal and coking coal, and the mass ratio of clean coal to coking coal is 1:1.
[0025] P2 iron ore powder: the main chemical composition is TFe 57.34%, SiO2 6.34%, CaO 0.13%, Al2O33.33%, MgO0.08%, TiO2 0.16%, P2O5 0.062%, S 0.034%, FeO 4.59%, LOI 10.7%, H2O9.98%; the particle size composition is 5.3% 10mm, 6.4% 8mm, 12.3% 5mm, 11.5% 3mm, 3.4% 2mm, 20.2% 1mm, 14.4% 0.5mm, 12.7% 0.25mm, 5.2% 0.125mm, 6.8% 0.063mm, 1.8% -0.063mm.
[0026] Jinbuba powder: The main chemical composition is H2O 8.10%, TFe 60.16%, CaO 0.02%, MgO 0.09%, SiO2 5.21%, Al2O3 2.96%, P 0.095%, TiO2 0.131%, S 0.028%, purchased from Wuan Changming Mining Materials Economic and Trade Co., Ltd.
[0027] Toke powder: The main chemical composition is H2O 9.70%, TFe 61.13%, CaO 0.22%, MgO 0.34%, SiO27.68%, Al2O3 1.56%, P 0.061%, TiO2 0.161%, S 0.027%, purchased from Wuan Changming Mining Materials Economic and Trade Co., Ltd.
[0028] Indian powder: The main chemical composition is H2O 9.10%, TFe 53.06%, FeO 0.38%, CaO 0.07%, MgO0.08%, SiO2 9.18%, Al2O3 4.43%, P0.08%, TiO 0.31%, S 0.03%, purchased from Wuan Changming Mining Materials Economic and Trade Co., Ltd.
[0029] WPF powder: The main chemical composition is H2O 6.10%, TFe 60.59%, CaO 0.01%, MgO 0.07%, SiO24.49%, Al2O3 2.43%, P 0.10%, TiO2 0.13%, S 0.03%.
[0030] Newman powder: The main chemical composition is H2O 8.80%, TFe 61.10%, CaO 0.08%, MgO 0.10%, SiO23.90%, Al2O3 2.38%, P 0.08%, TiO2 0.10%, S 0.03%, purchased from Wu'an Changming Mining Materials Economic and Trade Co., Ltd.
[0031] Mike powder: The main chemical composition is H2O 9.10%, TFe 60.49%, CaO 0.01%, MgO 0.10%, SiO24.23%, Al2O3 2.38%, P 0.07%, TiO2 0.09%, S 0.03%, purchased from Yushan Metallurgical Investment Co., Ltd.
[0032] Stone powder: The main chemical composition is CaO 47.63%, MgO 1.4%, SiO2 7.48%.
[0033] Example 1
[0034] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0035] S1. Weigh the components of the mixed ore powder according to Table 1 and set aside; the amount of return ore added is 20% of the total weight of all raw materials, and the amount of solid fuel added is 5.5% of the total weight of all raw materials;
[0036] S2, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; during the mixing process, add 8.5% of the total weight of the mixture and water, wherein the first mixer adds 80% of the total water, and the second mixer adds the remaining water;
[0037] S3. After sintering the mixed material, sintered ore is obtained; during the sintering process, the negative pressure of the flue is controlled at 14.0 KPa and the exhaust gas temperature is controlled at 120°C.
[0038] Example 2
[0039] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0040] S1. Weigh the components of the mixed ore powder according to Table 1 and set aside; the amount of return ore added is 20.5% of the total weight of all raw materials, and the amount of solid fuel added is 5.5% of the total weight of all raw materials;
[0041] S2, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; during the mixing process, add 8.0% of the total weight of the mixture and water, wherein the first mixer adds 80% of the total water added, and the second mixer adds the remaining water;
[0042] S3. After sintering the mixed material, sintered ore is obtained; during the sintering process, the negative pressure of the flue is controlled at 13.6 KPa and the exhaust gas temperature is controlled at 122°C.
[0043] Example 3
[0044] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0045] S1. Weigh the components of the mixed ore powder according to Table 1 and set aside; the amount of return ore added is 21% of the total weight of all raw materials, and the amount of solid fuel added is 5.5% of the total weight of all raw materials;
[0046] S2, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; during the mixing process, add 7.5% of the total weight of the mixture and water, wherein the first mixer adds 80% of the total water, and the second mixer adds the remaining water;
[0047] S3. After the mixed material is sintered, sintered ore is obtained; during the sintering process, the negative pressure of the flue is controlled at 13.2 KPa and the exhaust gas temperature is controlled at 125°C.
[0048] Example 4
[0049] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0050] S1. Weigh the components of the mixed ore powder according to Table 1 and set aside; the amount of return ore added is 23% of the total weight of all raw materials, and the amount of solid fuel added is 5.5% of the total weight of all raw materials;
[0051] S2, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; during the mixing process, add 7.8% of the total weight of the mixture and water, wherein the first mixer adds 80% of the total water, and the second mixer adds the remaining water;
[0052] S3. After the mixed material is sintered, sintered ore is obtained; during the sintering process, the negative pressure of the flue is controlled at 14.3 KPa and the exhaust gas temperature is controlled at 118°C.
[0053] Example 5
[0054] A method for preparing sintered ore containing P2 iron ore powder comprises the following steps:
[0055] S1. Weigh the components of the mixed ore powder according to Table 1 and set aside; the amount of return ore added is 23.7% of the total weight of all raw materials, and the amount of solid fuel added is 5.5% of the total weight of all raw materials;
[0056] S2, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; during the mixing process, add 8.0% of the total weight of the mixture and water, wherein the first mixer adds 80% of the total water added, and the second mixer adds the remaining water;
[0057] S3. After the mixed material is sintered, sintered ore is obtained; during the sintering process, the negative pressure of the flue is controlled at 14.6 KPa and the exhaust gas temperature is controlled at 115°C.
[0058] Table 1 Weight percentage of each component of mixed mineral powder in Examples 1-5 (%)
[0059]
[0060]
[0061] The drum index, 5-10 mm particle size ratio, utilization coefficient, and vertical sintering speed of the sintered ore prepared in Examples 1-5 were measured. The results are shown in Table 2.
[0062] Drum index: Take 20kg of finished sintered ore, put it into a drum, rotate it at 25 rpm for 4 minutes, then pour the sample onto a mechanical sieve with 5mm square holes and sieve it back and forth 10 times. The percentage of samples with a diameter larger than 5mm on the sieve to the total number of samples is the drum index.
[0063] Vertical sintering speed = material layer thickness / (sintering machine effective length / moving speed)
[0064] Utilization coefficient = sintering ore output (tons) / sintering machine area (m2 )*Actual operating time of sintering machine (hours)
[0065] Table 2 Measurement results
[0066]
[0067] In Examples 1-5, the proportion of P2 iron ore powder in the mixed ore powder is 15%, 20%, 25%, 30%, and 35%, respectively. It can be seen from Table 2 that when the proportion of P2 iron ore powder in Example 3 is 25%, the drum coefficient, utilization coefficient, vertical sintering speed, and low-temperature reduction pulverization index + 3.15 of the sintered ore are the highest, and the proportion of 5-10mm particle size is the smallest. Compared with Example 3, Examples 1, 2, 4, and 5 increase or decrease the proportion of P2 iron ore powder in the mixed ore powder, which will reduce the drum coefficient, utilization coefficient, vertical sintering speed, and low-temperature reduction pulverization index + 3.15 of the sintered ore, and increase the proportion of 5-10mm particle size. It shows that when the proportion of P2 iron ore powder in the mixed ore powder is 25%, the quality indicators of the sintered ore are the best.
[0068] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A sintered ore containing P2 iron ore powder, characterized in that: It includes the following components: mixed ore powder, return ore, flux, solid fuel; The mixed ore powder includes the following components: P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, Mike powder, stone powder; The solid fuel includes washed coal and coking coal; The mixed ore powder includes the following components by weight percentage: 25-35% P2 iron ore powder, 10-18% Jinbuba powder, 13-16% Tok powder, 10% India powder, 10-15% WPF powder, 10% Newman powder, 9-12% Mike powder, and 2-4% stone powder; The main chemical composition of the P2 iron ore powder is TFe 57.34%, SiO2 6.34%, CaO 0.13%, Al2O3 3.33%, MgO 0.08%, TiO2 0.16%, P2O5 0.062%, S 0.034%, FeO 4.59%, LOI 10.7%, H2O 9.98%; The particle size composition of the P2 iron ore powder is 5.3% 10mm, 6.4% 8mm, 12.3% 5mm, 11.5% 3mm, 3.4% 2mm, 20.2% 1mm, 14.4% 0.5mm, 12.7% 0.25mm, 5.2% 0.125 mm, 6.8% 0.063mm, and 1.8% -0.063mm.
2. The sintered ore containing P2 iron ore powder according to claim 1, characterized in that: The mixed ore powder includes the following components by weight percentage: 25% P2 iron ore powder, 13% Jinbuba powder, 16% Tok powder, 10% India powder, 10% WPF powder, 10% Newman powder, 12% Mike powder, and 4% stone powder.
3. The sintered ore containing P2 iron ore powder according to claim 1, characterized in that: The added amount of the return ore is 20-23.7% of the total weight of all raw materials.
4. The sintered ore containing P2 iron ore powder according to claim 1, characterized in that: The added amount of the solid fuel is 5.5% of the total weight of all raw materials.
5. The method for preparing sintered ore containing P2 iron ore powder according to claim 1, characterized in that: The following steps are involved: S1, after mixing P2 iron ore powder, Jinbuba powder, Tok powder, India powder, WPF powder, Newman powder, and Mike powder, add return ore, solid fuel, and stone powder, and send them to the sintering machine through the first mixer and the second mixer for uniform mixing to obtain a mixture; S2. Sintering the mixed material to obtain sintered ore.
6. The method for preparing sintered ore containing P2 iron ore powder according to claim 5, characterized in that: During the sintering process in step S2, the negative pressure of the flue is 13.2-14.6 KPa, and the exhaust gas temperature is 115-125°C.
7. The method for preparing sintered ore containing P2 iron ore powder according to claim 5, characterized in that: In step S1, 7.5-8.5% of the total weight of the mixture and water is added during the mixing process, wherein 80% of the total water is added in the first mixing and the remaining water is added in the second mixing.