A leveling agent for pulse hole filling electroplating of printed circuit boards and its application

By using a leveling agent prepared by reacting aromatic nitrile derivatives with sodium azide in pulse-filled electroplating of printed circuit boards, combining specific accelerators and carriers, a high-temperature and oxidation-resistant electroplating solution was formed, and the current solution was solved. There are problems of low pore filling rate and high production cost in the technology, and efficient blind hole filling and low-cost production are achieved.

CN115717258BActive Publication Date: 2024-11-15上海天承化学有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211582938.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-15
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

In the prior art, the leveling agent used for pulse-filling electroplating of printed circuit boards is difficult to work effectively in high salt content and high temperature environments, resulting in low pore filling rate and high production cost, and is incompatible with fine line production.

Method used

Provide a leveling agent for pulse-filling electroplating of printed circuit boards, prepared by reacting aromatic nitrile derivatives with sodium azide, and combined with specific accelerators and carriers to form a high temperature and oxidation-resistant electroplating liquid. , suitable for high salt content copper sulfate pulse plating tanks.

Benefits of technology

It improves the blind hole filling effect, reduces the porosity of the plating and the internal stress of the plating, reduces the amount of additives, reduces the process cost, and is compatible with fine line production, improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115717258B_ABST
    Figure CN115717258B_ABST
Patent Text Reader

Abstract

The present invention provides a leveling agent for pulse hole filling electroplating of a printed circuit board and its application. When the leveling agent provided by the present invention is used in a copper electroplating solution, it has a good blind hole filling effect, can ensure that the blind hole filling plating meets conventional requirements, and can reduce the porosity and internal stress of the plating layer, reduce the amount of additives, and reduce the impurity content in the plating layer. The electroplating solution added with the leveling agent of the present invention has the advantages of high temperature resistance and oxidation resistance, is suitable for use on a pulse electroplating line, and is suitable for a copper sulfate pulse electroplating tank with a high salt content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating, and in particular relates to a leveling agent used for pulse hole-filling electroplating of a printed circuit board and application thereof. Background Art

[0002] In order to improve the mechanical strength, wiring density, heat dissipation performance, electrical signal performance, etc. of printed circuit boards (PCB or PWB), there are a large number of micro blind vias in high-density (HDI) circuit boards, and these blind vias need to be filled with electroplated copper. There are two main electroplating methods currently adopted. One is to use a DC power supply to electroplating copper to fill the blind holes in an electroplating tank with copper sulfate as the main salt. Most of this electroplating process is completed on a gantry line or a VCP electroplating line; the other is to use a pulse power supply to electroplating copper to fill the blind holes. This electroplating process is almost completed on a horizontal electroplating line. Due to the special anode structure and distribution, extremely small distance between the anode and cathode, and special design of the jet and nozzle in the horizontal electroplating line, a pulse power supply can be used to fill the blind holes with high current density, with good filling effect and thin copper plating layer on the board surface. For many years, the horizontal electroplating line equipment and chemical liquid technology in each process have been monopolized by foreign companies, resulting in huge investment by PCB manufacturers and excessively high production costs.

[0003] In the horizontal line pulse electroplating copper tank, in addition to the high content of the main salt copper sulfate, it also contains a large amount of other salt substances, which are easy to crystallize at room temperature, causing nozzles and pipelines to be blocked. Therefore, the production line generally adopts 35-40 degrees of insulation maintenance, which is far higher than the normal use temperature of DC electroplating copper additives (22-28 degrees). In addition, this type of electroplating copper tank contains a certain concentration of trivalent iron ions during electroplating. The iron ions have a certain oxidation effect on the additives, causing the loss of the effective ingredients of the additives. The presence of iron ions especially accelerates the failure of biological dyes such as Jianna Green B. Therefore, electroplating additives suitable for this horizontal electroplating line, high copper sulfate content, iron ion content, high current density, long-term high temperature use, and easy automatic analysis and automatic addition control have always been the technical core of foreign companies. The additives used in this environment include accelerators, carriers, leveling agents, etc. Among them, the leveling agent has always been a technical barrier that is difficult to break through due to its extremely small dosage and vague electrochemical reaction mechanism.

[0004] CN105018977A discloses a hole-filling electroplating leveler and a preparation method thereof and an electroplating solution using the hole-filling electroplating leveler, and relates to the field of electroplating technology. The hole-filling electroplating leveler comprises ingredients 3-(dimethylamino)-1-propanethiol, piperazine, and a divalent epoxy compound. The hole-filling electroplating leveler of the invention improves the interaction between the leveler molecule and the accelerator and inhibitor by introducing a sulfur-containing functional group into the leveler molecule, so that the three types of additives cooperate better with each other, thereby enabling the prepared electroplating solution to achieve excellent hole-filling performance.

[0005] CN110158124A discloses a copper electroplating leveler molecule and an electroplating solution using the same. The copper electroplating leveler molecule is a nitrogen-containing compound that can be adsorbed at the blind hole during the copper electroplating process. The copper electroplating leveler of the present invention is applied to the electroplating solution to achieve copper surface leveling, prevent hole openings from being vacant, and increase the relevant hole filling rate to 91-99%. The copper surface thickness is 10-13 μm.

[0006] However, after the integrator obtained by the above-mentioned prior art is applied to the plating solution, the plating solution is not suitable for pulse plating. Therefore, it is necessary to develop a leveling agent suitable for pulse hole filling plating of printed circuit boards to increase the blind hole filling rate after pulse plating, thereby improving the leveling effect. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a leveling agent for pulse hole filling electroplating of printed circuit boards and its application.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a leveler for pulse hole filling electroplating of a printed circuit board, the structure of the leveler comprising:

[0010] , or ,

[0011] Wherein Ar represents a benzene ring or a naphthalene ring;

[0012] R is independently selected from any one of hydrogen, halogen, thiol, nitro, hydroxyl, aldehyde, C1-10 alkyl, and C1-8 alkoxy;

[0013] n is independently any integer from 1 to 5 (eg, 1, 2, 3, 4 or 5).

[0014] When the leveling agent provided by the present invention is used in an electro-copper plating solution, it has a good blind hole filling effect, can ensure that the blind hole filling and plating meet conventional requirements, can reduce the porosity and internal stress of the plating layer, reduce the amount of additives, and reduce the impurity content in the plating layer. The use of the leveling agent of the present invention can not only improve production efficiency, but also reduce process costs, and has excellent compatibility with the production of fine circuits, reducing the difficulty of subsequent etching of fine circuits.

[0015] Preferably, the aldehyde group is selected from a formaldehyde group or an acetaldehyde group.

[0016] Preferably, the C1-10 alkyl group is selected from any one of methyl, ethyl or n-propyl.

[0017] Preferably, the C1-8 alkoxy group is selected from any one of methoxy, ethoxy or octoxy.

[0018] Preferably, the leveler is obtained by reacting an aromatic nitrile derivative with sodium azide;

[0019] Preferably, the molar ratio of the aromatic nitrile derivative to sodium azide is 1:1-1.3, for example, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5 or 1:2.8, etc.

[0020] Preferably, the reaction of the aromatic nitrile derivative with sodium azide is carried out at a constant temperature.

[0021] Preferably, the reaction temperature is 120-130°C, and the reaction time is 3-4h. For example, the reaction temperature may be 121°C, 122°C, 123°C, 124°C, 125°C, 126°C, 127°C, 128°C or 129°C, and the reaction time may be 3.1h, 3.2h, 3.3h, 3.4h, 3.5h, 3.6h, 3.7h, 3.8h or 3.9h, etc.

[0022] Preferably, a catalyst needs to be added during the reaction.

[0023] Preferably, the catalyst is iodine.

[0024] Preferably, the amount of the catalyst is 0.8%-1.2% of the amount of the aromatic nitrile derivative, for example, it can be 0.8%, 0.9%, 1%, 1.1% or 1.2%.

[0025] Specific point values ​​within the above numerical ranges can be selected and will not be described in detail here.

[0026] In a second aspect, the present invention provides a use of the leveler as described in the first aspect in pulse hole filling electroplating of a printed circuit board.

[0027] In a third aspect, the present invention provides an electroplating solution, wherein the electroplating solution includes a leveler for pulse hole filling electroplating of a printed circuit board as described in the first aspect.

[0028] Preferably, the electroplating solution comprises the following components in terms of mass concentration:

[0029] Copper sulfate pentahydrate 180-300g / L

[0030] 98% sulfuric acid 30-100g / L

[0031] Chloride ion 0.03-0.12g / L

[0032] Iron ion 1-20g / L

[0033] Accelerator 0.0005-0.025 g / L

[0034] Carrier 0.05-1.5 g / L

[0035] The leveling agent as described in the first aspect is 0.0005-0.015 g / L.

[0036] In the present invention, the electroplating solution added with the leveling agent described in the first aspect has the advantages of high temperature resistance and oxidation resistance, is suitable for use on a pulse electroplating line, and is suitable for a copper sulfate pulse electroplating tank with a high salt content.

[0037] The mass concentration of the copper sulfate pentahydrate in the electroplating solution of the present invention can be 190 g / L, 200 g / L, 210 g / L, 220 g / L, 230 g / L, 240 g / L, 250 g / L, 260 g / L, 270 g / L, 280 g / L or 290 g / L, etc.;

[0038] The mass concentration of the 98% sulfuric acid can be 35 g / L, 40 g / L, 45 g / L, 50 g / L, 55 g / L, 60 g / L, 65 g / L, 70 g / L, 75 g / L, 80 g / L, 85 g / L, 90 g / L or 95 g / L, etc.;

[0039] The mass concentration of chloride ions refers to the mass concentration based on the mass of chlorine element, for example, it can be 0.04 g / L, 0.05 g / L, 0.06 g / L, 0.07 g / L, 0.08 g / L, 0.09 g / L, 0.1 g / L or 0.11 g / L, etc.;

[0040] The mass concentration of iron ions refers to the mass concentration based on the mass of the iron element, for example, it can be 2 g / L, 4 g / L, 6 g / L, 8 g / L, 10 g / L, 12 g / L, 14 g / L, 16 g / L or 18 g / L, etc.;

[0041] The mass concentration of the accelerator can be 0.0007 g / L, 0.001 g / L, 0.005 g / L, 0.01 g / L, 0.012 g / L, 0.015 g / L, 0.018 g / L, 0.02 g / L, 0.022 g / L or 0.024 g / L, etc.;

[0042] The mass concentration of the carrier can be 0.05 g / L, 0.1 g / L, 0.3 g / L, 0.5 g / L, 0.7 g / L, 0.9 g / L, 1 g / L, 1.2 g / L or 1.4 g / L, etc.;

[0043] The mass concentration of the leveling agent as described in the first aspect can be 0.0007 g / L, 0.0009 g / L, 0.001 g / L, 0.005 g / L, 0.01 g / L, 0.012 g / L or 0.014 g / L, etc.

[0044] Preferably, the iron ion provider includes soluble iron-containing inorganic salts and their derivatives, or inorganic iron salts and their derivatives soluble under electrolytic conditions.

[0045] Preferably, the iron ion provider includes ferric sulfate and / or ferric chloride.

[0046] Preferably, the mass concentration of the iron ions is 1.5-10 g / L.

[0047] Preferably, the chloride ion provider includes chloride salt and / or hydrochloric acid.

[0048] Preferably, the chloride salt comprises potassium chloride and / or sodium chloride.

[0049] Preferably, the accelerator includes any one of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate, sodium N,N-dimethyldithiocarboxamide propane sulfonate, or a combination of at least two thereof.

[0050] Preferably, the accelerator is a combination of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate.

[0051] As a preferred technical solution of the present invention, when the accelerator is a combination of the above three components, it can be better adsorbed on the copper surface, reduce the electrochemical reaction potential of the electroplating reaction, promote rapid deposition reaction, and make the growth rate of the crystal surface tend to be uniform, forming a coating with a dense structure and neat directional arrangement.

[0052] Preferably, the mass ratio of the sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate is 1:(0.1-0.8):(0.1-1).

[0053] Where "0.1-0.8" can be 0.2, 0.3, 0.4, 0.5, 0.6 or 0.7, etc.;

[0054] “0.1-1” can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc.

[0055] Preferably, the carrier comprises polyethylene glycol with a molecular weight of 3000-20000, for example, the molecular weight may be 5000, 7000, 9000, 10000, 12000, 14000, 16000 or 18000, etc.

[0056] Preferably, the carrier is a combination of polyethylene glycol 10000, polyethylene glycol 8000 and polyethylene glycol 4000.

[0057] In the present invention, when the carrier is a combination of polyethylene glycol 10000, polyethylene glycol 8000, and polyethylene glycol 4000, it can better inhibit the reduction of copper ions, thereby promoting uniform adsorption of the leveling agent, reducing the surface tension of the electronic plating solution, and improving the density of the coating.

[0058] Preferably, the mass ratio of polyethylene glycol 10000, polyethylene glycol 8000 and polyethylene glycol 4000 is 1:(0.1-1):(0.1-0.6).

[0059] Where "0.1-1" can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc.;

[0060] “0.1-0.6” can mean 0.1, 0.2, 0.3, 0.4, 0.5 or 0.6, etc.

[0061] Specific point values ​​within the above numerical ranges can be selected and will not be described in detail here.

[0062] In a fourth aspect, the present invention provides an electroplating method of the electroplating solution as described in the third aspect, the electroplating method comprising the following steps:

[0063] The printed circuit board with blind holes is subjected to chemical copper plating, acid immersion, and then immersed in the electroplating solution as described in the third aspect to perform pulse electroplating.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] (1) When the leveling agent provided by the present invention is used in the electro-copper plating solution, it has a good blind hole filling effect, which can not only ensure that the blind hole filling and plating meet the conventional requirements, but also reduce the porosity and internal stress of the plating layer, reduce the amount of additives, and reduce the impurity content in the plating layer. The use of the leveling agent of the present invention can not only improve production efficiency, but also reduce process costs, and has excellent compatibility with the production of fine circuits, reducing the difficulty of subsequent etching of fine circuits.

[0066] (2) The electroplating solution of the present invention can have the advantages of high temperature resistance and oxidation resistance by adding a specific leveling agent, and is suitable for use on a pulse electroplating line and is suitable for a copper sulfate pulse electroplating tank with a high salt content. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 This is the slicing effect after the electroplating of Application Example 1 is completed;

[0068] Figure 2 This is the slicing effect after the electroplating of Application Example 2 is completed;

[0069] Figure 3 This is the slicing effect after the electroplating of Application Example 3 is completed;

[0070] Figure 4 This is the slicing effect after the electroplating of Application Example 4 is completed;

[0071] Figure 5 This is the slicing effect after the electroplating is completed in the comparative application example 1;

[0072] Figure 6 This is the slicing effect after the electroplating is completed in the comparative application example 2; DETAILED DESCRIPTION

[0073] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0074] Some of the materials and source information involved in the following examples and comparative examples are as follows:

[0075]

[0076] The rest of the raw materials can be used as long as they are purchased from regular dealers.

[0077] Example 1

[0078] This embodiment provides a leveling agent for pulse hole filling electroplating of printed circuits, and the preparation method of the leveling agent is as follows:

[0079] In a 100 ml three-necked flask equipped with a reflux condenser and a thermometer, add 40 ml of 5% ammonia water and 12.6 g of p-methylbenzonitrile, stir under magnetic force at room temperature to dissolve, add 0.1 g of iodine and 6.7 g of sodium azide to the flask after dissolution, heat to 120 degrees in an oil bath, reflux condensate, react for 4 hours under stirring to obtain a light yellow liquid, and then use an appropriate amount of 5% sodium thiosulfate to remove the iodine in the product. Place the liquid obtained from the final reaction on a watch glass and evaporate to obtain a white to light yellow solid, which is the synthesized leveling agent. The structural formula of the leveling agent is as follows:

[0080]

[0081] Example 2

[0082] This embodiment provides a leveling agent for pulse hole filling electroplating of printed circuits, and the preparation method of the leveling agent is as follows:

[0083] In a 100 ml three-necked flask equipped with a reflux condenser and a thermometer, add 40 ml of 5% ammonia water and 17.2 g of 2-ethoxybenzonitrile, stir under magnetic force at room temperature to dissolve, add 0.15 g of iodine and 6.7 g of sodium azide to the flask after dissolution, heat to 150 degrees in an oil bath, react for 4 hours under reflux condensation and stirring to obtain a light yellow liquid, and then use an appropriate amount of 5% sodium thiosulfate to remove the iodine in the product. The liquid obtained from the final reaction is placed on a watch glass and evaporated to obtain a white to light yellow solid, which is the synthesized leveling agent. The structural formula of the leveling agent is as follows:

[0084]

[0085] Example 3

[0086] This embodiment provides a leveling agent for pulse hole filling electroplating of printed circuits, and the preparation method of the leveling agent is as follows:

[0087] In a 100 ml three-necked flask equipped with a reflux condenser and a thermometer, add 40 ml of 5% ammonia water and 18.2 g of 1-naphthonitrile, stir under magnetic force at room temperature to dissolve, add 0.15 g of iodine and 7.2 g of sodium azide to the flask after dissolution, heat to 150 degrees in an oil bath, react for 4 hours under reflux condensation and stirring to obtain a light yellow liquid, and then use an appropriate amount of 5% sodium thiosulfate to remove the iodine in the product. The liquid obtained from the final reaction is placed on a watch glass to evaporate, and a white to light yellow solid is obtained, which is the synthesized leveling agent. The structural formula of the leveling agent is as follows:

[0088]

[0089] Example 4

[0090] This embodiment provides a leveling agent for pulse hole filling electroplating of printed circuits, and the preparation method of the leveling agent is as follows:

[0091] In a 100 ml three-necked flask equipped with a reflux condenser and a thermometer, add 40 ml of 5% ammonia water and 25.2 g of 3-phenoxybenzyl cyanide, stir under magnetic force at room temperature to dissolve, add 0.15 g of iodine and 8.5 g of sodium azide to the flask after dissolution, heat to 135 degrees in an oil bath, react for 4 hours under reflux condensation and stirring to obtain a light yellow liquid, and then use an appropriate amount of 5% sodium thiosulfate to remove the iodine in the product. The liquid obtained from the final reaction is placed on a watch glass and evaporated to obtain a white to light yellow solid, which is the synthesized leveling agent. The structural formula of the leveling agent is as follows:

[0092]

[0093] Application Example 1

[0094] This application example provides an electroplating solution, which includes the following components according to mass concentration: 275 g / L copper sulfate pentahydrate, 50 g / L 98% sulfuric acid, 0.07 g / L sodium chloride (chloride ion concentration), 10 g / L iron sulfate (iron ion concentration), 1.2 mg / L accelerator, 1 g / L carrier, and 1.5 mg / L leveler obtained in Example 1;

[0095] The accelerator is a combination of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2:1:1;

[0096] The carrier is a combination of polyethylene glycol 10000, polyethylene glycol 8000 and polyethylene glycol 4000 in a mass ratio of 1:0.5:0.3.

[0097] Application Example 2-4

[0098] This application example provides four electroplating solutions. The difference between the electroplating solutions and application example 1 is that the leveling agent obtained in example 1 is replaced with an equal amount of leveling agents obtained in examples 2-4, and the other components and contents remain unchanged.

[0099] The electroplating method used is referred to Application Example 1.

[0100] Application Example 5

[0101] This application example provides an electroplating solution, the electroplating solution differing from Application Example 1 only in that the accelerator is a combination of sodium polydisulfide propane sulfonate and sodium 3-mercapto-1-propane sulfonate in a mass ratio of 2:1, and the amount of the accelerator added is kept unchanged, while the other components and their contents remain unchanged.

[0102] The electroplating method used is referred to Application Example 1.

[0103] Application Example 6

[0104] This application example provides an electroplating solution, the electroplating solution differing from Application Example 1 only in that the accelerator is a combination of sodium polydisulfide propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate in a mass ratio of 2:1, and the amount of the accelerator added is kept unchanged, while the other components and contents remain unchanged.

[0105] The electroplating method used is referred to Application Example 1.

[0106] Application Example 7

[0107] This application example provides an electroplating solution, the electroplating solution differing from Application Example 1 only in that the accelerator is a 1:1 combination of sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithioformamide propane sulfonate, and the amount of the accelerator added remains unchanged, while the other components and their contents remain unchanged.

[0108] The electroplating method used is referred to Application Example 1.

[0109] Application Example 8

[0110] This application example provides an electroplating solution, the difference between the electroplating solution and application example 1 is that the carrier is a combination of polyethylene glycol 10000 and polyethylene glycol 8000 in a mass ratio of 2:1, and the added amount of the carrier is kept unchanged, and the other components and contents remain unchanged.

[0111] The electroplating method used is referred to Application Example 1.

[0112] Application Example 9

[0113] This application example provides an electroplating solution, the difference between the electroplating solution and application example 1 is that the carrier is a combination of polyethylene glycol 10000 and polyethylene glycol 4000 in a mass ratio of 1:0.3, and the added amount of the carrier is kept unchanged, and the other components and contents remain unchanged.

[0114] The electroplating method used is referred to Application Example 1.

[0115] Application Example 10

[0116] This application example provides an electroplating solution, the difference between the electroplating solution and application example 1 is that the carrier is a combination of polyethylene glycol 8000 and polyethylene glycol 4000 in a mass ratio of 5:3, and the added amount of the carrier is kept unchanged, and the other components and contents remain unchanged.

[0117] The electroplating method used is referred to Application Example 1.

[0118] Comparative application example 1

[0119] This application example provides an electroplating solution. The electroplating solution is different from the application example 1 only in that the leveling agent in the embodiment 1 is replaced by Janus Green B of the same mass concentration, and the other components and proportions remain unchanged. The structure of Janus Green B is as follows:

[0120]

[0121] Comparative Application Example 2

[0122] This application example provides an electroplating solution. The difference between the electroplating solution and application example 1 is that the leveling agent in embodiment 1 is replaced by benzotriazole of the same mass concentration, and the other components and proportions remain unchanged. The structure of the benzotriazole is as follows:

[0123]

[0124] Performance Testing

[0125] The electroplating solutions of Application Examples 1-10 and Comparative Application Examples 1-2 were tested as follows, and the method included:

[0126] A FR4 board with a thickness of 1.0 mm and blind holes with a diameter of 100 microns and a depth of 60 microns on both sides was electroplated to obtain a bottom copper layer with a thickness of 0.4 microns, and then acid-immersed (10% sulfuric acid solution, room temperature, 1 minute) and flash-plated to thicken the coating to 5 microns. In a pulse electroplating copper bath containing the electroplating solution described in Examples 1-10 and Comparative Examples 1-2, at 40°C, the pulse current setting in Table 1 was used to electroplate and fill the above PCB blind holes for 30 minutes.

[0127] Table 1

[0128]

[0129] (1) Blind hole filling effect:

[0130] Take the blind hole position of the PCB board after the above electroplating to make a slice, and use the BX53MTRF-S Olympus metallographic microscope to observe the filling effect at 200 times. After electroplating for 30 minutes, the pit depth (Dimple) after the blind hole is filled is less than 10 microns, and the surface copper plating layer thickness does not exceed 15 microns to be qualified.

[0131] (2) Stability of leveling agent

[0132] In the continuous production state, according to the electrolytic amount of the plating solution (kiloampere-hours), the leveling agent consumption in the plating solution is analyzed by the CVS instrument to judge the stability of the leveling agent. The judgment criteria are shown in Table 2:

[0133] Table 2

[0134]

[0135] The test results are summarized in Table 3.

[0136] Table 3

[0137]

[0138] Analysis of the data in Table 1 shows that the electroplating solution of the present invention has a good filling effect after adding a specific leveling agent, and the effective amount of the leveling agent used is also relatively low. The consumption of the leveling agent in Application Examples 1-4 is less than 0.5 mg / KAH. At the same time, it has a good blind hole filling effect, the Dimple value is below 2.5 microns, and the thickness of the surface copper plating layer is below 10 microns.

[0139] By analyzing and comparing Application Example 1 with Application Examples 5-7 and 8-10, it can be seen that the types of carrier and accelerator also affect the blind hole filling effect after electroplating. Specifically, in Application Example 5-7, when the type of accelerator changes, the Dimple value after blind hole filling is 4.6-5.9 microns, and the thickness of the surface copper plating layer is 11.3-13.6 microns; in Application Examples 8-10, when the type of carrier changes, the Dimple value after blind hole filling is 5.8-7.2 microns, and the thickness of the surface copper plating layer is 7.5-10.2 microns. Compared with Example 1, the blind hole effect is reduced.

[0140] From the analysis of Application Example 1 and Comparative Application Examples 1-2, it can be seen that when the integration agent is not of the structure specified in the present application, the effect of blind hole filling is significantly poor, and the amount of leveling agent used is also significantly increased.

[0141] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the leveling agent for pulse hole filling electroplating of printed circuit boards and its application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0142] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0143] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. An electroplating solution, characterized in that: The components of the electroplating solution include a leveling agent; The structure of the leveling agent includes: , or , Wherein Ar represents a benzene ring or a naphthalene ring; R is independently selected from any one of hydrogen, halogen, thiol, nitro, hydroxyl, aldehyde, C1-10 alkyl, and C1-8 alkoxy; n is independently any integer from 1 to 5; The aldehyde group is selected from a formaldehyde group or an acetaldehyde group; The C1-10 alkyl group is selected from any one of methyl, ethyl or n-propyl; The C1-8 alkoxy group is selected from any one of methoxy, ethoxy or octoxy.

2. The electroplating solution according to claim 1, characterized in that The electroplating solution comprises the following components according to mass concentration: Copper sulfate pentahydrate 180-300g / L 98% sulfuric acid 30-100g / L Chloride ion 0.03-0.12g / L Iron ion 1-20g / L Accelerator 0.0005-0.025 g / L Carrier 0.05-1.5 g / L Leveling agent 0.0005-0.015 g / L; The accelerator includes any one of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate, sodium N,N-dimethyldithiocarboxamide propane sulfonate, or a combination of at least two thereof; The carrier includes polyethylene glycol with a molecular weight of 3000-20000.

3. The electroplating solution according to claim 2, characterized in that The iron ion provider includes ferric sulfate and / or ferric chloride.

4. The electroplating solution according to claim 2, characterized in that: The mass concentration of the iron ions is 1.5-10 g / L.

5. The electroplating solution according to claim 2, characterized in that The chloride ion provider includes chloride salt and / or hydrochloric acid.

6. The electroplating solution according to claim 5, characterized in that The chloride salt includes potassium chloride and / or sodium chloride.

7. The electroplating solution according to claim 2, characterized in that: The accelerator is a combination of sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate.

8. The electroplating solution according to claim 7, characterized in that The mass ratio of the sodium polydisulfide propane sulfonate, sodium 3-mercapto-1-propane sulfonate and sodium N,N-dimethyldithiocarboxamide propane sulfonate is 1:(0.1-0.8):(0.1-1).

9. The electroplating solution according to claim 2, characterized in that: The carrier is a combination of polyethylene glycol 10000, polyethylene glycol 8000 and polyethylene glycol 4000.

10. The electroplating solution according to claim 9, characterized in that The mass ratio of polyethylene glycol 10000, polyethylene glycol 8000 and polyethylene glycol 4000 is 1:(0.1-1):(0.1-0.6).

11. The electroplating method of the electroplating solution according to any one of claims 1 to 10, characterized in that: The electroplating method comprises the following steps: The printed circuit board with blind holes is subjected to chemical copper plating, acid immersion, and then immersed in the electroplating solution described in any one of claims 1 to 10 for pulse electroplating.