A method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure

By coating nanoferric oxide with phenolic resin and forming a graphitized carbon shell, combined with optimized processing by magnetic decantation, a carbon-coated nanoscale zero-valent iron material with a core-shell structure was prepared, which solved the problem of the ease of nanoscale zero-valent iron. It solves the problems of agglomeration and oxidation, achieves efficient oxidative degradation of organic pollutants, and achieves the effects of simple process and production expansion.

CN115722666BActive Publication Date: 2024-10-01NANJING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211540241.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-10-01
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The application of nanoscale zero-valent iron in the field of environmental remediation is limited by its easy agglomeration and oxidation problems, and the existing preparation methods are complex and difficult to produce on a large scale, and there is a lack of effective carbon-coated core-shell structural materials.

Method used

Phenolic resin is used to coat nano-ferric oxide, and a graphitized carbon shell is formed through high-temperature carbothermal reduction. Combined with optimized processing by magnetic decantation, a carbon-coated nano zero-valent iron material with a core-shell structure is prepared.

Benefits of technology

The anti-oxidation and electron transfer capabilities of nano-zero-valent iron have been improved, and it can be used as an efficient persulfate activator for the oxidative degradation of organic pollutants in water, and the process is simple and can be expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115722666B_ABST
    Figure CN115722666B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure, comprising the following steps: S1: weighing a phenolic substance and dissolving it in anhydrous ethanol and water, adding nano ferroferric oxide microspheres, and dispersing them under ultrasonic conditions; S2: adding ammonia water and formaldehyde to the mixed solution in sequence, mechanically stirring the reaction at 30°C for 1h, treating the mixed solution by magnetic decantation, washing the magnetic fluid mixture to neutrality, obtaining solid particles, and drying to obtain a nano ferroferric oxide composite material coated with phenolic resin; S3: placing the nano ferroferric oxide composite material in a tubular furnace and calcining it at 750-950°C to obtain a carbon-coated core-shell nano zero-valent iron composite material. The composite material prepared by the method of the invention has high antioxidant capacity and excellent electron transfer capacity due to the protection and isolation of the external graphitized carbon shell layer, and can be used as an efficient persulfate activator for efficient oxidative degradation of organic pollutants in water bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental restoration, and in particular to a method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure. Background Art

[0002] Nano-zero-valent iron has attracted extensive attention in the field of environmental remediation due to its advantages such as environmental friendliness, low price, large specific surface area and high reactivity. Based on its strong reducibility, nano-zero-valent iron can be directly used to remove heavy metals, halogen compounds and nitro compounds in the environment. In the field of advanced oxidation, nano-zero-valent iron can be used as a highly active persulfate activator for the oxidative removal of various difficult-to-degrade organic pollutants. However, due to its own magnetism and high surface energy, nano-zero-valent iron is easy to agglomerate, which reduces its electron transfer ability and activity. In addition, nano-zero-valent iron easily reacts with oxygen in the air, making its storage and transportation difficult, limiting its large-scale practical application.

[0003] At present, porous materials such as activated carbon, biomass carbon, and carbon nanotubes are usually used as carriers of nano zero-valent iron to reduce its agglomeration. However, since nano zero-valent iron is loaded on the surface of the material, it is easy to fall off, and the oxidation problem of nano zero-valent iron is also difficult to solve effectively. Studies have shown that embedding nano zero-valent iron inside other materials to form a nano zero-valent iron composite material with a core-shell structure can effectively slow down its oxidation process. At present, the most research is on sulfide nano zero-valent iron, which has good reactivity and selectivity, as well as good electron transfer ability. It is considered to be a type of environmental remediation material with practical application prospects. The lack of adsorption capacity and space for structural regulation is the main problem facing sulfide nano zero-valent iron.

[0004] Compared with sulfur, carbon-coated nano zero-valent iron has more advantages. The carbon layer is easy to modify with functional groups and the pore structure is easy to control. Studies have shown that the carbon layer can achieve pre-enrichment of pollutants through adsorption, and the special surface properties of carbon, especially graphitized carbon, can promote electron transfer at the interface of the material. If a graphitized carbon-coated nano zero-valent iron composite material with a core-shell structure can be prepared, it will be expected to solve the aggregation and oxidation problems of nano zero-valent iron at the same time and obtain excellent electron transfer ability. However, there are currently few studies on carbon-coated core-shell nano zero-valent iron composite materials. Most of the preparation methods involve long hydrothermal reactions, complex processes, difficult to accurately control, and difficult to mass produce. Therefore, developing a simple method for large-scale preparation of nano zero-valent iron composite materials with a core-shell structure has become an important research topic. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure.

[0006] The technical solution of the present invention is:

[0007] A method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure comprises the following steps:

[0008] S1, ultrasonic dispersion: weigh 1-5 parts by weight of phenolic substances, dissolve them in a mixed solution consisting of 20 parts by weight of anhydrous ethanol and 50 parts by weight of water, then add 1 part by weight of nano-iron tetroxide microspheres to the mixed solution, and disperse the mixed solution under ultrasonic conditions for 10-15 minutes;

[0009] S2, stirring reaction: adding ammonia water and 1-10 parts by weight of formaldehyde to the mixed solution obtained in step S1 in sequence, so that the molar concentration of ammonia in the mixed solution is 0.1-0.5 mol / L, then mechanically stirring the mixed solution at 30° C. for 1 hour, and then treating the mixed solution by magnetic decantation to obtain a magnetic fluid mixture, washing the magnetic fluid mixture with deionized water until neutral to obtain solid particles, and then drying the solid particles to obtain a phenolic resin-coated nano-iron tetroxide composite material;

[0010] S3, high temperature calcination: placing the nano-iron tetroxide composite material obtained in step S2 in a tubular furnace, filling it with inert gas for protection and calcining it at 750-950° C. for 5-6 hours to obtain a carbon-coated core-shell nano-zero-valent iron composite material.

[0011] Furthermore, the phenolic substance in step S1 is one or two of phenol, resorcinol, hydroquinone and phloroglucinol. The selected phenolic substances are all phenolic compounds that are easy to react with formaldehyde to generate phenolic resin.

[0012] Furthermore, the particle size of the nano-ferroferric oxide microspheres is 20-100 nm. The best reaction effect can be achieved by selecting nano-ferroferric oxide microspheres with appropriate particle sizes.

[0013] Furthermore, the rotation speed of the mechanical stirring in step S2 is 200-300 rpm. The stirring speed is adjusted to ensure that the phenolic substance and formaldehyde react completely.

[0014] Furthermore, the method for treating the mixed solution by magnetic decantation in step S2 is: subjecting the mixed solution to magnetic decantation treatment through a magnetic decantation component, removing the supernatant of the mixed solution to obtain a lower layer of magnetic fluid liquid, then mixing the lower layer of magnetic fluid liquid with deionized water at a weight ratio of 1:5, and subjecting the mixed solution to magnetic decantation treatment through a magnetic decantation component again, repeating the magnetic decantation treatment three times, and finally obtaining a magnetic fluid mixture;

[0015] The magnetic decantation assembly comprises a magnetic decantation barrel, a base located at the bottom of the magnetic decantation barrel, a cover plate is provided at the front end of the magnetic decantation barrel, the cover plate and the bottom of the magnetic decantation barrel are both provided with slots, a sliding baffle is provided at the front end of the cover plate and is slidably connected to the slots, a magnet is provided at the bottom of the rear end of the sliding baffle and is slidably connected to the bottom of the magnetic decantation barrel, a liquid level baffle is provided at the upper part of the rear end of the sliding baffle and is slidably connected to the bottom of the inner wall of the magnetic decantation barrel, a sealing plate for sealing the slots is provided at the rear end of the magnet, the sealing plate slides and is sealedly connected to the bottom of the magnetic decantation barrel, a fixing block is provided at the rear end of the sealing plate, a fixing groove for accommodating the sealing plate and slidably connected to the sealing plate is provided at the front end of the fixing block, the bottom of the fixing block is fixedly connected to the base, the top of the fixing block is fixedly connected to the magnetic decantation barrel, and a water inlet is provided at the top of the magnetic decantation barrel;

[0016] A slide rail is provided on each side of the upper surface of the base, and a slide groove is provided on the inner wall of the slide rail. A slide rod is provided in the slide groove for sliding connection. The slide rod is fixedly connected to the front end of the sealing plate and is used to drive the sealing plate, the magnet and the sliding baffle to slide. A telescopic motor is provided at the front end of the slide rail, and the output end of the telescopic motor is connected to the slide rod to push the slide rod to move. A drainage groove is provided in the middle of the upper surface of the base, and the drainage groove extends from the position of the rear end of the groove to the front end of the base. A stirring motor is provided in the middle of the rear end of the magnetic decantation barrel. The output end of the stirring motor passes through the magnetic decantation barrel and is connected to a stirring rod located in the middle of the magnetic decantation barrel. The stirring rod is provided with several groups of stirring blades, and the stirring range of the stirring blades has the lowest end located above the liquid level baffle. By providing a magnetic decantation assembly, the rapid magnetic decantation process of the magnetic fluid mixture can be completed, thus avoiding waste of resources and improving extraction efficiency.

[0017] Furthermore, in step S2, the method of washing the magnetic fluid mixture with deionized water until it is neutral is as follows: placing the magnetic fluid mixture in a centrifuge and centrifuging it at 3000-3500 rpm for 15-20 min to obtain a centrifuged mixture, washing the mixture with deionized water, repeating the centrifugation process three times, and obtaining the final solid particles by repeating the centrifugation process three times. Other impurities in the solid particles can be effectively removed by centrifugation combined with the magnetic decantation method.

[0018] Furthermore, the method of drying the solid particles in step S2 is: vacuum drying the solid particles at 70-80° C. for 12 hours. The drying time and temperature are adjusted to ensure that the drying process does not affect the properties of the solid particles.

[0019] Furthermore, the inert gas in step S3 is argon. The selected argon is a common protective gas.

[0020] Furthermore, the carbon-coated core-shell nano zero-valent iron composite material obtained in step S3 is applied to the advanced oxidation degradation process of organic pollutants in water by persulfate activator. BP-1 selected here has carcinogenic effect and endocrine disrupting effect, which is widely present in various water bodies, and it is difficult to completely remove it by conventional treatment methods in sewage treatment plants.

[0021] The beneficial effects of the present invention are:

[0022] (1) The preparation method of the carbon-coated nano zero-valent iron material with a core-shell stable structure of the present invention utilizes phenolic resin to coat ferroferric oxide nanoparticles, combined with high-temperature carbon thermal reduction under the protection of inert gas, to carbonize the phenolic resin to form a carbon shell layer while reducing the ferroferric oxide in situ to nano zero-valent iron. The obtained carbon-coated core-shell nano zero-valent iron composite material has a carbon coating layer thickness of 10 to 50 nm. The prepared composite material has high antioxidant capacity and excellent electron transfer capacity due to the protection and isolation of the external graphitized carbon shell layer. This nano zero-valent iron composite material with a unique structure can be used as a very efficient persulfate activator for the efficient oxidation degradation of organic pollutants in water bodies.

[0023] (2) The preparation method of the carbon-coated nano zero-valent iron material with a core-shell stable structure of the present invention provides an improved and optimized magnetic decantation component by optimizing the magnetic decantation method and combining the physical and chemical properties of the phenolic resin-coated nano ferroferric oxide composite material, which can complete the rapid magnetic decantation treatment process of the magnetic fluid mixture, avoid resource waste, and improve the extraction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 For SEM and TEM characterization of materials, Figure 1 A is a scanning electron microscope image of the phenolic resin-based carbon material RF-C in the experimental example of the present invention, Figure 1 B is a scanning electron microscope image of commercial nano-iron tetroxide in the experimental example of the present invention, Figure 1 C~F are Fe 0 @RF-C-1#'s SEM image, EDS image, and two high-resolution TEM images;

[0025] Figure 2 Fe in the experimental examples of the present invention 0 @RF-C-1# structural evaluation drawing group, Figure 2 A~F are respectively Fe 0 @RF-C-1#'s X-ray diffraction diagram, X-ray surface photoelectron spectrum, Raman spectrum, N2 adsorption-desorption isotherm diagram, pore size distribution diagram, and hysteresis loop diagram;

[0026] Figure 3Fe in the experimental examples of the present invention 0 @The variation curve of BP-1 removal efficiency over time in the mixed system of RF-C-1# and PS and the systems of comparative examples 1-6;

[0027] Figure 4 Fe in the experimental examples of the present invention 0 @Degradation kinetics of BP-1 by RF-C-1# and commercial nano zero-valent iron activated PS exposed to air for different days;

[0028] Figure 5 The degradation kinetics of BP-1 by activated PS of the carbon-coated core-shell nano zero-valent iron composite material prepared in Example 1-3 of the experimental example of the present invention;

[0029] Figure 6 The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite prepared in Examples 1, 4-6 of the present invention;

[0030] Figure 7 The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite prepared in Examples 1, 7, and 8 of the present invention;

[0031] Figure 8 The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials prepared in Examples 1, 9, and 10 of the present invention are shown;

[0032] Fig. 9 The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite prepared in Examples 1, 11 and 12 of the present invention;

[0033] Fig.10 The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite prepared in Examples 1, 13 and 14 of the present invention;

[0034] Fig.11 It is a schematic diagram of the structure of the magnetic decantation assembly of the present invention;

[0035] Fig.12 This is a schematic diagram of the bottom structure of the magnetic decantation assembly of the present invention after omitting the base;

[0036] Fig.13 It is a schematic diagram of the internal structure of the magnetic decantation barrel of the magnetic decantation assembly of the present invention;

[0037] Fig.14 It is a schematic diagram of the bottom structure of the magnetic decantation assembly of the present invention after the magnet moves.

[0038] Among them, 1-magnetic decantation barrel, 11-cover plate, 12-slot, 13-sliding baffle, 14-water inlet, 2-base, 21-drainage groove, 3-magnet, 4-liquid level baffle, 5-sealing plate, 6-fixed block, 61-fixed groove, 7-slide rail, 71-slide groove, 72-slide rod, 73-telescopic motor, 8-stirring motor, 81-stirring rod, 82-stirring blade. DETAILED DESCRIPTION Example 1

[0039] A method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure comprises the following steps:

[0040] S1, ultrasonic dispersion: weigh 2 parts by weight of a phenolic substance, the phenolic substance is resorcinol, dissolve it in a mixed solution consisting of 20 parts by weight of anhydrous ethanol and 50 parts by weight of water, then add 1 part by weight of nano-iron tetroxide microspheres to the mixed solution, the particle size of the nano-iron tetroxide microspheres is 20 nm, and disperse the mixed solution under ultrasonic conditions for 12 minutes;

[0041] S2, stirring reaction: adding ammonia water and 4 parts by weight of formaldehyde to the mixed solution obtained in step S1 in sequence, so that the molar concentration of ammonia in the mixed solution is 0.25 mol / L, then mechanically stirring the mixed solution at 30° C. for 1 hour, the speed of the mechanical stirring is 250 rpm, and then treating the mixed solution by magnetic decantation to obtain a magnetic fluid mixture, washing the magnetic fluid mixture with deionized water until neutral, obtaining solid particles, and then drying the solid particles to obtain a phenolic resin-coated nano-iron tetroxide composite material;

[0042] The method for treating the mixed solution by magnetic decantation is as follows: the mixed solution is subjected to magnetic decantation treatment by a magnetic decantation component, the supernatant of the mixed solution is removed to obtain a lower layer of magnetic fluid liquid, the lower layer of magnetic fluid liquid is then mixed with deionized water at a weight ratio of 1:5, and the mixed solution is subjected to magnetic decantation treatment by the magnetic decantation component again, the magnetic decantation treatment is repeated three times, and finally a magnetic fluid mixture is obtained, wherein the magnetic decantation component is a commercially available magnetic decantation component;

[0043] The method of washing the magnetic fluid mixture with deionized water to neutrality is as follows: placing the magnetic fluid mixture in a centrifuge and centrifuging it at 3200 rpm for 18 minutes to obtain a centrifuged mixture, washing the mixture with deionized water, repeating the centrifugation process three times, and obtaining the three centrifuged mixtures is the final solid particles;

[0044] The method of drying the solid particles is as follows: vacuum drying the solid particles at 75°C for 12 hours;

[0045] S3, high temperature calcination: the nano-iron oxide composite material obtained in step S2 is placed in a tube furnace, filled with argon gas for protection and calcined at 850°C for 5.5h to obtain a carbon-coated core-shell nano zero-valent iron composite material, named Fe 0 @RF-C-1#. Example 2

[0046] S1, ultrasonic dispersion: weigh 2 parts by weight of a phenolic substance, the phenolic substance is resorcinol, dissolve it in a mixed solution consisting of 20 parts by weight of anhydrous ethanol and 50 parts by weight of water, then add 1 part by weight of nano-iron tetroxide microspheres to the mixed solution, the particle size of the nano-iron tetroxide microspheres is 50 nm, and disperse the mixed solution under ultrasonic conditions for 10 minutes;

[0047] S2, stirring reaction: adding ammonia water and 4 parts by weight of formaldehyde to the mixed solution obtained in step S1 in sequence, so that the molar concentration of ammonia in the mixed solution is 0.25 mol / L, then mechanically stirring the mixed solution at 30° C. for 1 hour, the speed of the mechanical stirring is 200 rpm, and then treating the mixed solution by magnetic decantation to obtain a magnetic fluid mixture, washing the magnetic fluid mixture with deionized water until neutral, obtaining solid particles, and then drying the solid particles to obtain a phenolic resin-coated nano-iron tetroxide composite material;

[0048] The method for treating the mixed solution by magnetic decantation is as follows: the mixed solution is subjected to magnetic decantation treatment by a magnetic decantation component, the supernatant of the mixed solution is removed to obtain a lower layer of magnetic fluid liquid, the lower layer of magnetic fluid liquid is then mixed with deionized water at a weight ratio of 1:5, and the mixed solution is subjected to magnetic decantation treatment by the magnetic decantation component again, the magnetic decantation treatment is repeated three times, and finally a magnetic fluid mixture is obtained, wherein the magnetic decantation component is a commercially available magnetic decantation component;

[0049] The method of washing the magnetic fluid mixture with deionized water to neutrality is as follows: placing the magnetic fluid mixture in a centrifuge and centrifuging it at 3000 rpm for 15 minutes to obtain a centrifuged mixture, washing the mixture with deionized water, repeating the centrifugation process three times, and obtaining the three centrifuged mixtures is the final solid particles;

[0050] The method of drying the solid particles is as follows: vacuum drying the solid particles at 70°C for 12 hours;

[0051] S3, high temperature calcination: The nano-iron oxide composite material obtained in step S2 is placed in a tube furnace, filled with argon gas for protection and calcined at 850°C for 5 hours to obtain a carbon-coated core-shell nano zero-valent iron composite material, named Fe 0 @RF-C-2#. Example 3

[0052] S1, ultrasonic dispersion: weigh 2 parts by weight of a phenolic substance, the phenolic substance is resorcinol, dissolve it in a mixed solution consisting of 20 parts by weight of anhydrous ethanol and 50 parts by weight of water, then add 1 part by weight of nano-iron tetroxide microspheres to the mixed solution, the particle size of the nano-iron tetroxide microspheres is 100 nm, and disperse the mixed solution under ultrasonic conditions for 10 minutes;

[0053] S2, stirring reaction: adding ammonia water and 4 parts by weight of formaldehyde to the mixed solution obtained in step S1 in sequence, so that the molar concentration of ammonia in the mixed solution is 0.25 mol / L, then mechanically stirring the mixed solution at 30° C. for 1 hour, the speed of the mechanical stirring is 300 rpm, and then treating the mixed solution by magnetic decantation to obtain a magnetic fluid mixture, washing the magnetic fluid mixture with deionized water until neutral, obtaining solid particles, and then drying the solid particles to obtain a phenolic resin-coated nano-iron tetroxide composite material;

[0054] The method for treating the mixed solution by magnetic decantation is as follows: the mixed solution is subjected to magnetic decantation treatment by a magnetic decantation component, the supernatant of the mixed solution is removed to obtain a lower layer of magnetic fluid liquid, the lower layer of magnetic fluid liquid is then mixed with deionized water at a weight ratio of 1:5, and the mixed solution is subjected to magnetic decantation treatment by the magnetic decantation component again, the magnetic decantation treatment is repeated three times, and finally a magnetic fluid mixture is obtained, wherein the magnetic decantation component is a commercially available magnetic decantation component;

[0055] The method of washing the magnetic fluid mixture with deionized water to neutrality is as follows: placing the magnetic fluid mixture in a centrifuge and centrifuging it at 3500 rpm for 20 minutes to obtain a centrifuged mixture, washing the mixture with deionized water, repeating the centrifugation process three times, and obtaining the three centrifuged mixtures is the final solid particles;

[0056] The method of drying the solid particles is as follows: vacuum drying the solid particles at 70°C for 12 hours;

[0057] S3, high temperature calcination: The nano-iron oxide composite material obtained in step S2 is placed in a tube furnace, filled with argon gas for protection and calcined at 850°C for 6 hours to obtain a carbon-coated core-shell nano zero-valent iron composite material, named Fe 0 @RF-C-3#. Example 4

[0058] The difference between this embodiment and embodiment 1 is that:

[0059] The phenolic substance in step S1 is phenol, and the carbon-coated core-shell nano zero-valent iron composite material is obtained in step S3, which is named Fe 0 @RF-C-4#. Example 5

[0060] The difference between this embodiment and embodiment 1 is that:

[0061] The phenolic substance in step S1 is hydroquinone, and the carbon-coated core-shell nano zero-valent iron composite material is obtained in step S3, which is named Fe 0 @RF-C-5#. Example 6

[0062] The difference between this embodiment and embodiment 1 is that:

[0063] The phenolic substance in step S1 is phloroglucinol, and the carbon-coated core-shell nano zero-valent iron composite material is obtained in step S3, which is named Fe 0 @RF-C-6#. Example 7

[0064] The difference between this embodiment and embodiment 1 is that:

[0065] The molar concentration of ammonia in the mixed solution in step S2 is 0.1 mol / L. In step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-7#. Example 8

[0066] The difference between this embodiment and embodiment 1 is that:

[0067] The molar concentration of ammonia in the mixed solution in step S2 is 0.5 mol / L. In step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-8#. Example 9

[0068] The difference between this embodiment and embodiment 1 is that:

[0069] In step S1, 1 part by weight of phenolic substances is weighed, and ammonia water and 2 parts by weight of formaldehyde are added to the mixed solution obtained in step S2 in sequence, and in step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-9#. Example 10

[0070] The difference between this embodiment and embodiment 1 is that:

[0071] In step S1, 5 parts by weight of phenolic substances are weighed, and ammonia water and 10 parts by weight of formaldehyde are added to the mixed solution obtained in step S2 in sequence. In step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-10#. Embodiment 11

[0072] The difference between this embodiment and embodiment 1 is that:

[0073] In step S1, 2 parts by weight of phenolic substances are weighed, and ammonia and 2 parts by weight of formaldehyde are added to the mixed solution obtained in step S2 in sequence, and in step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-11#. Example 12

[0074] The difference between this embodiment and embodiment 1 is that:

[0075] In step S1, 2 parts by weight of phenolic substances are weighed, and ammonia water and 10 parts by weight of formaldehyde are added to the mixed solution obtained in step S2 in sequence, and in step S3, a carbon-coated core-shell nano zero-valent iron composite material is obtained, which is named Fe 0 @RF-C-12#. Embodiment 13

[0076] The difference between this embodiment and embodiment 1 is that:

[0077] The calcination temperature in step S3 is 750°C to obtain a carbon-coated core-shell nano zero-valent iron composite material, named Fe 0 @RF-C-13#. Embodiment 14

[0078] The difference between this embodiment and embodiment 1 is that:

[0079] The calcination temperature in step S3 is 950°C to obtain a carbon-coated core-shell nano zero-valent iron composite material, named Fe 0 @RF-C-14#. Embodiment 15

[0080] This embodiment is an optimization of the magnetic decantation assembly in Embodiment 1.

[0081] like Fig.11 , 12As shown, the magnetic decantation assembly includes a magnetic decantation barrel 1, a base 2 located at the bottom of the magnetic decantation barrel 1, a cover plate 11 is provided at the front end of the magnetic decantation barrel 1, and a slot 12 is provided at the cover plate 11 and the bottom of the magnetic decantation barrel 1. A sliding baffle 13 is provided at the front end of the cover plate 11 and is slidably connected to the slot 12. A magnet 3 is provided at the bottom of the rear end of the sliding baffle 13 and is slidably connected to the bottom of the magnetic decantation barrel 1. A liquid level baffle 4 is provided at the upper part of the rear end of the sliding baffle 13 and is slidably connected to the bottom of the inner wall of the magnetic decantation barrel 1. The rear end of the magnet 3 is provided with a sealing groove 12. 2, the sealing plate 5 is slidably and sealedly connected to the bottom of the magnetic decantation barrel 1, a fixing block 6 is provided at the rear end of the sealing plate 5, a fixing groove 61 for accommodating the sealing plate 5 and slidably connected to the sealing plate 5 is provided at the front end of the fixing block 6, the bottom of the fixing block 6 is fixedly connected to the base 2, the top of the fixing block 6 is fixedly connected to the magnetic decantation barrel 1, a water inlet 14 is provided at the top of the magnetic decantation barrel 1, and the front and rear ends of the magnetic decantation barrel 1 are both provided with auxiliary fixing brackets, and the fixing bracket and the bottom surface of the base are located at the same horizontal plane, which is not shown in the figure;

[0082] like Fig.13 , 14 As shown, a slide rail 7 is provided on each side of the upper surface of the base 2, and a slide groove 71 is provided on the inner wall of the slide rail 7. A slide rod 72 is provided in the slide groove 71 for sliding connection. The slide rod 72 is fixedly connected to the front end of the sealing plate 5 and is used to drive the sealing plate 5, the magnet 3 and the sliding baffle 13 to slide. A telescopic motor 73 is provided at the front end of the slide rail 7, and the output end of the telescopic motor 73 is connected to the slide rod 72 to push the slide rod 72 to move. A drainage groove 21 is provided in the middle of the upper surface of the base 2, and the drainage groove 21 extends from the rear end of the slot 12 to the front end of the base 2. A stirring motor 8 is provided in the middle of the rear end of the magnetic decantation barrel 1. The output end of the stirring motor 8 passes through the magnetic decantation barrel 1 and is connected to a stirring rod 81 located in the middle of the magnetic decantation barrel 1. A plurality of groups of stirring blades 82 are provided on the stirring rod 81, and the lower end of the stirring range of the stirring blade 82 is located above the liquid level baffle 4.

[0083] The working principle of the magnetic decantation assembly is briefly described below in conjunction with the method of step S3:

[0084] When in use, first inject the mixed solution into the magnetic decantation barrel 1 through the water inlet 14, turn on the stirring motor 8 to drive the stirring rod 81 to rotate, so that the mixed solution is stirred by the stirring blade 82, and then turn on the telescopic motor 73 so that its output end pushes the sliding rod 72 to slide along the sliding groove 71, thereby driving the sealing plate 5, the magnet 3 and the sliding baffle 13 to slide, so that the magnet 3 continuously attracts the solid particles in the mixed solution during the stirring process until the sliding baffle 13 slides to the slot 12 of the cover plate 11. At this time, the position of the magnet 3 is located in the middle of the magnetic decantation barrel 1, and the drainage begins. The discharged liquid flows out through the drainage groove 21 for recovery, and the magnet 3 is continued to be moved until the position of the magnet 3 is located at the rear end of the magnetic decantation barrel 1, and the sliding rod 72 contacts the fixed block 6. Fig.14As shown, at this time, the solution inside the magnetic decantation barrel 1 has been completely discharged, and the liquid level height in the magnetic decantation barrel 1 is maintained at the position of the liquid level baffle 4, to obtain the lower layer of magnetic fluid liquid, and after resetting each structural member, the lower layer of magnetic fluid liquid is taken out and then the lower layer of magnetic fluid liquid is mixed with deionized water at a weight ratio of 1:5, and the magnetic decantation treatment is performed again through the magnetic decantation component, and the magnetic decantation treatment is repeated three times to finally obtain a magnetic fluid mixture. Example 16

[0085] This example applies the carbon-coated core-shell nano zero-valent iron composite material obtained in Example 1 to the advanced oxidation degradation process of organic pollutants in water using a persulfate activator.

[0086] In order to evaluate the performance of the carbon-coated core-shell nano zero-valent iron composite material, the carbon-coated core-shell nano zero-valent iron composite material was used as a persulfate (PS) activator, and an organic pollutant with great environmental harm, UV filter 2,4-dihydroxybenzophenone (BP-1), was selected as the target pollutant, and its degradation process in the persulfate system was studied in depth. The BP-1 selected here has carcinogenic and endocrine disrupting effects. It is widely present in various water bodies. It is difficult to completely remove it by conventional treatment methods in sewage treatment plants. Of course, other pollutants can also be selected as treatment objects, especially those pollutants that are more harmful to the environment, difficult to degrade, and widely concerned by people.

[0087] After the composite material and the BP-1 aqueous solution are fully mixed, a certain amount of persulfate is added for oxidation reaction. After a certain period of time, a sample is taken and the reaction is immediately quenched with methanol. The concentration of BP-1 in the sample is analyzed by high performance liquid chromatography to determine its degradation rate.

[0088] Experimental example

[0089] In order to better understand the present invention, the carbon-coated core-shell nano zero-valent iron composite materials prepared under different conditions (ferroferric oxide particle size, type of phenol, amount of phenol and aldehyde added, calcination temperature) in Examples 1 to 14 were used as PS activators to investigate the degradation effect of BP-1 in aqueous solution.

[0090] The degradation experiment process of BP-1 is as follows: 5 mg of the composite material is added to 100 mL of BP-1 (20 μM, pH = 5.00 ± 0.10) aqueous solution at 30 ° C, and the mixture is thoroughly stirred. Then, 100 μL of sodium persulfate aqueous solution (1 M) is added while stirring to start the degradation reaction. After a specific time interval, 1 mL of the sample is taken and immediately added to 1 mL of methanol to quench the reaction. The sample is filtered through a PTFE filter into a liquid vial, and the concentration of BP-1 in the sample is analyzed by high performance liquid chromatography, and its removal rate is calculated.

[0091] HPLC test conditions: Agilent 1260 high performance liquid chromatograph, XDB-C18 (5µm, 4.6×250mm, Agilent, USA) column, UV detector, detection wavelength 350nm, mobile phase methanol / 0.3% formic acid water (70 / 30), flow rate 1mL min-1, column 30°C.

[0092] In order to illustrate the activation effect of the carbon-coated core-shell nano zero-valent iron composite material prepared by the present invention on PS, a phenolic resin-based carbon material (named RF-C) without the addition of ferroferric oxide was prepared according to the same method, and the degradation of BP-1 in the systems of commercial nano-Fe3O4, RF-C, carbon-coated core-shell nano zero-valent iron composite material and PS, and Fe3O4 / PS and RF-C / PS mixed systems were investigated respectively.

[0093] The preparation method of RF-C is the same as the preparation process of step S1 in Example 1 of the present invention, except that nano-iron tetroxide microspheres are not added during the preparation process.

[0094] Comparative Example 1: Adsorption experiment of BP-1 by nano-ferroferric oxide system alone

[0095] Similar to the above BP-1 degradation experiment, only nano-Fe3O4 was added during the experiment, and PS was not added. That is, 5 mg of nano-Fe3O4 was added to 100 mL of BP-1 (20 μM, pH = 5.00 ± 0.10) aqueous solution at 30 ° C and stirred. After a specific time interval, 1 mL of the sample was taken and immediately added to 1 mL of methanol. The concentration of BP-1 in the sample was analyzed by HPLC, and its removal rate was calculated.

[0096] Comparative Example 2: Adsorption experiment of BP-1 by phenolic resin-based carbon material system alone

[0097] Similar to the above BP-1 degradation experiment process, only RF-C was added during the experiment, and PS was not added.

[0098] Comparative Example 3: Adsorption experiment of BP-1 by single carbon-coated core-shell nano zero-valent iron composite system

[0099] Similar to the above-mentioned degradation experimental process of BP-1, only the carbon-coated core-shell nano zero-valent iron composite material was added during the experiment, and PS was not added.

[0100] Comparative Example 4: Degradation experiment of BP-1 by PS system alone

[0101] Similar to the above-mentioned degradation experimental process of BP-1, only PS was added during the experiment, and no other materials were added.

[0102] Comparative Example 5: Degradation experiment of BP-1 by ferroferric oxide and PS composite system

[0103] Similar to the above-mentioned degradation experimental process of BP-1, PS and ferrosoferric oxide were added during the experiment.

[0104] Comparative Example 6: Degradation experiment of BP-1 by phenolic resin-based carbon material and PS composite system

[0105] Similar to the above BP-1 degradation experiment, PS and RF-C were added during the experiment.

[0106] 1. Characterization of Carbon-Coated Core-Shell Nano-Zerovalent Iron Composites

[0107] The prepared carbon-coated core-shell nano zero-valent iron composite material was first characterized in terms of structure, morphology, composition and specific surface area. The specific characterization content, characterization instruments and conditions are as follows:

[0108] Scanning electron microscope analysis: SSX-550 scanning electron microscope (equipped with EDS energy spectrum), scanning voltage 10kV, the sample surface was gold-sprayed before testing to increase its conductivity.

[0109] Transmission electron microscopy analysis: The analysis was carried out using a JEM-2100 high-resolution transmission electron microscope.

[0110] XRD determination: Bruker D8A dvance X-ray powder diffractometer, scanning speed 5° / min, scanning range 5~90°, scanning mode theta / 2theta, scanning mode continue, tube voltage 40kV, tube current 40mA, Cu target Kα ray (λ=1.54178Å).

[0111] XPS analysis: Thermo Fischer ESCALAB 250XI X-ray photoelectron spectrometer was used for analysis.

[0112] Raman analysis: The analysis was performed using a Lab RAMA ramis (HJY, Paris, France) laser confocal Raman spectrometer at an excitation wavelength of 532 nm.

[0113] Surface area analysis: Micromeritics ASAP 2020-M+C surface area analyzer, 50-100 mg of sample was activated at 90°C for 24h and then backfilled with N2. Then the N2 adsorption-desorption isotherm was measured under liquid nitrogen (77K). The BET method provided by the instrument was used to calculate the surface area of ​​the material.

[0114] Hysteresis loop analysis: Quantum Design PPMS Dyna Cool MPMS XL-7 magnetometer was used for analysis at 300K.

[0115] Iron content analysis: The iron content in the sample was analyzed by combustion method. 20 mg of the sample was calcined in a muffle furnace at 600°C in an air environment for 6 hours to completely convert the iron into Fe2O3. The iron content in the sample was calculated based on the mass before and after calcination.

[0116] The characterization results of the carbon-coated core-shell nano zero-valent iron composite material are illustrated by taking the composite material prepared in Example 1 as an example and comparing it with the prepared RF-C and the purchased nano ferroferric oxide particles.

[0117] Figure 1 For SEM and TEM characterization of materials. Figure 1 A shows that RF-C is composed of irregular particles with obvious stacking pores. Figure 1 B shows that the purchased nano Fe3O4 particles are spherical, with smooth surface and particle size ranging from several hundred nanometers to 2 microns. Figure 1 C can be seen that the Fe prepared by the present invention 0 @RF-C-1# is also spherical, with a particle size similar to its precursor nano-Fe3O4, but its surface is rougher. Figure 1 EDS analysis of D showed that most of the Fe 0 @RF-C-1# The surface is covered with carbon layer. Figure 1 E can clearly see Fe 0 @RF-C-1# core-shell structure, shell thickness is about 20nm. Figure 1 Fe can be seen in F 0 Lattice fringes of graphitic carbon and zero-valent iron in @RF-C-1# (the fringe spacing corresponds to 0.36nm and 0.20nm, respectively).

[0118] Figure 2 A is Fe 0 @RF-C-1#'s XRD spectrum shows Fe 0 @RF-C-1# has diffraction peaks at 2θ of 44.9°, 65.3° and 82.5°, which are consistent with the standard diffraction peak position of zero-valent iron. No diffraction peak of ferroferric oxide was found, indicating that ferroferric oxide has been completely reduced to zero-valent iron at high temperature. In addition, a diffraction peak belonging to graphitized carbon can be found at 2θ of 26.3°, indicating that the carbon in the shell has a partial graphitized structure.

[0119] Figure 2B is the XPS spectrum of Fe2p. Overall, the absorption peak of Fe2p is very weak, indicating that most of the iron is wrapped inside the carbon layer. The absorption peaks at the binding energy of 710.5eV and 723.6eV are the characteristic peaks of Fe2p3 / 2 and Fe2p1 / 2. These absorption peaks can be further divided into the Fe2p1 / 2 absorption peaks at 722.3eV and 725.0eV and the Fe2p3 / 2 absorption peaks at 709.5eV and 711.9eV. Among them, the absorption peaks at 709.5eV and 722.3eV belong to Fe2+, and the absorption peaks at 711.9eV and 725.0eV belong to Fe3+. No absorption peak of zero-valent iron was found at 707.2eV, indicating that there is no zero-valent iron on the surface of the material, which may be because the small amount of zero-valent iron exposed is easily oxidized by air.

[0120] Figure 2 C is the Raman spectrum of Fe0@RF-C-1# and RF-C. The two peaks at 1350cm-1 and 1580cm-1 belong to the D band and the G band, corresponding to amorphous carbon and graphitized carbon, respectively. The ratio of the peak area of ​​the D band and the G band (ID / IG) reflects the degree of graphitization of carbon. 0 The ID / IG values ​​in the Raman spectra of @RF-C-1# and RF-C are 2.65 and 2.72, respectively, indicating that the materials formed a partially graphitized carbon structure during the calcination process.

[0121] Combined with SEM, TEM, EDS, XRD, XPS and Raman spectroscopy, it shows that Fe 0 @RF-C-1# is a composite material with a core-shell structure, with zero-valent iron inside and partially graphitized carbon wrapped on the outside.

[0122] Depend on Figure 2 D can be seen that Fe 0 The N2 adsorption-desorption isotherm of @RF-C-1# has an obvious desorption hysteresis loop in the range of P / P0=0.4–1.0, indicating that it has a certain mesoporous structure. According to the BET model, Fe 0 @RF-C-1# has a specific surface area of ​​143m 2 g -1 . Figure 2 E is Fe obtained based on the desorption data based on the BJH method 0 @RF-C-1# pore size distribution curve. It can be seen that the composite material has a concentrated pore distribution at 3.9nm.

[0123] The combustion method was used to analyze Fe 0 The iron content of @RF-C-1# is 54.9%.

[0124] Figure 2 F is ferroferric oxide, nano zero-valent iron and Fe 0 @RF-C-1# hysteresis loop. All samples have typical S-type hysteresis loops at room temperature, with no remanence and coercivity, indicating that they have superparamagnetism. 0 The saturation magnetization intensities of @RF-C-1# are 57.56, 199.34 and 93.43emug respectively. -1 Due to the presence of the surface carbon layer, Fe 0 The magnetic properties of @RF-C-1# are weaker than those of nano zero-valent iron. However, after being dispersed in water, Fe 0 @RF-C-1# can also be easily separated in the presence of an external magnetic field.

[0125] 2. Degradation of BP-1 in water by persulfate activated by carbon-coated core-shell nano-zero-valent iron composites

[0126] BP-1 was selected as the target pollutant and its Fe 0 @RF-C-1# and PS mixed system to evaluate the degradation kinetics of Fe 0 @RF-C-1# activation performance on PS. In addition, the BP-1 removal experiment in the above comparative example was carried out under the same experimental conditions for comparison.

[0127] like Figure 3 As shown, in Comparative Examples 1, 2 and 3, the removal rates of BP-1 after 40 minutes of reaction were 3.4%, 9.1% and 13.4%, respectively, which indicates that the contribution of adsorption to the removal of BP-1 is small. In Comparative Example 4, the removal rate of BP-1 after 40 minutes of reaction was only 3.6%, indicating that the direct oxidation effect of PS on BP-1 can be ignored and it is difficult to be activated at room temperature. After 40 minutes of reaction, in Comparative Examples 5 and 6, the removal rates of BP-1 were only 7.5% and 9.0%, respectively, indicating that neither RF-C nor Fe3O4 can effectively activate PS at room temperature. Obviously, in Example 1, the removal rate of BP-1 increased significantly to 94.9% within 10 minutes, indicating that Fe 0 @RF-C-1# can effectively activate PS at room temperature. Combining the above experimental results, it can be concluded that in Fe 0 @ In the RF-C-1# / PS mixed system, direct oxidation of PS and Fe 0 The adsorption of @RF-C-1# did not play a leading role in the removal of BP-1, while Fe 0 @RF-C-1# The catalytic oxidation of BP-1 by activated PS is the main reason for its efficient removal.

[0128] Fe 0The porous carbon layer on the outside of @RF-C-1# is conducive to the adsorption of BP-1 and the diffusion of PS, which allows BP-1 to be enriched on the surface of the material and shortens the contact distance between it and the generated free radicals, thus promoting the degradation of BP-1. In addition, the graphitized carbon layer structure promotes the transfer of electrons in the system, thereby improving the removal effect of BP-1.

[0129] 3. Stability evaluation of carbon-coated core-shell nano-zero-valent iron composites in air

[0130] In order to evaluate the stability of the carbon-coated core-shell nano zero-valent iron composite material in air, the Fe prepared in Example 1 was 0 @RF-C-1# was exposed to air for 40 days, and some materials were taken on the 5th and 40th days respectively, and the performance of its activated PS degradation of BP-1 was investigated according to the above method. During the experiment, we also selected commercial nano zero-valent iron as a comparison under the same experimental conditions.

[0131] like Figure 4 As shown, freshly prepared Fe 0 @RF-C-1# showed a high PS activation ability, and more than 90% of BP-1 was degraded within 5 minutes. The material Fe obtained after 5 days and 40 days of exposure to air 0 @RF-C-1#-5d and Fe 0 @RF-C-1#-40d has similar activation ability to PS, although it is comparable to freshly prepared Fe 0 @RF-C-1# is slightly lower than that of BP-1, but the degradation rate of BP-1 is more than 90% within 10 minutes, which shows that the carbon-coated core-shell nano zero-valent iron composite material prepared by the present invention has high stability in the air. Fresh commercial nano zero-valent iron also showed a high PS activation ability, and more than 80% of BP-1 was degraded within 10 minutes. However, after exposure to air for 5 days, the activation performance of the obtained material nZVI-5d for PS decreased significantly. After 30 minutes of reaction, the degradation rate of BP-1 was less than 70%, while only 14.6% of BP-1 was degraded at 10 minutes of reaction. After 40 days of exposure to air, the activation ability of the obtained material nZVI-40d for PS was similar to that of nZVI-5d, but slightly reduced. The experimental results show that commercial nano zero-valent iron is very easy to be oxidized in the air, resulting in a serious decrease in the ability to activate PS. Due to the protection of the external carbon layer, the carbon-coated core-shell nano zero-valent iron composite material prepared by the present invention has high stability in the air.

[0132] 4. Comparison of the degradation effects of persulfate activated carbon-coated core-shell nano zero-valent iron composite materials on BP-1 in different embodiments

[0133] The degradation kinetics of BP-1 by the activated PS of the composite materials of Examples 1-3 are as follows: Figure 5 . It can be seen that the composite materials prepared from nano-ferroferric oxide of different particle sizes all showed a high PS activation ability, and the degradation rate of BP-1 in all embodiments within 30 minutes reached 95%. In addition, the composite material prepared with 20nm nano-ferroferric oxide as raw material has the best performance, and the degradation rate of BP-1 in Example 1 can reach 90% at 5 minutes. With the increase of the particle size of nano-ferroferric oxide, the activation performance of the prepared composite material on PS decreases slightly. This may be because under the same conditions, the larger the particle size, the smaller the area of ​​contact between the material and PS and BP-1, thereby slowing down the reaction rate.

[0134] The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials of Examples 1 and 4-6 are as follows: Figure 6 The activation performance of composite materials prepared using different phenols as raw materials on PS is not much different, and the degradation rate of BP-1 in all corresponding examples is more than 90% at 10 min. We believe that the benzene ring structure of phenols itself is conducive to the formation of graphitized carbon in the subsequent carbon thermal reduction process. Since the phenolic resins prepared from different phenols contain a large amount of benzene ring structure, it does not show a significant effect on the performance of the final composite material.

[0135] The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials of Examples 1, 7 and 8 are as follows: Figure 7 . There is no significant difference in the activation performance of PS for composite materials prepared under different ammonia concentrations. BP-1 in all corresponding examples can be quickly degraded, and its degradation rate exceeds 90% within 10 minutes. Different ammonia concentrations will only affect the generation rate of phenolic resin, and will not affect the reaction mechanism, nor the carbon layer structure on the surface of the final material. Therefore, the ammonia concentration has little effect on the material preparation process. Although the ammonia concentration range studied in the present invention is 0.10-0.50 mol·L -1 However, this does not mean that other ammonia concentrations are inappropriate. During the material preparation process, the reaction conditions and costs should be considered comprehensively to select the appropriate ammonia concentration.

[0136] The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials of Examples 1, 9 and 10 are as follows: Figure 8. The composite materials prepared by different phenol dosages have obvious differences in PS activation performance. Too high or too low phenol dosage is not conducive to obtaining composite materials with high PS activation performance. In Example 1, the composite material prepared when the mass ratio of phenol to ferroferric oxide is 2:1 has the best activation performance for PS, and the degradation rate of BP-1 within 5min is more than 90%. In the same time, the degradation rates of BP-1 in Examples 9 and 10 are 82.3% and 80.2% respectively. The dosage of phenol determines the thickness of the phenolic resin coating on the surface of ferroferric oxide, and ultimately determines the thickness of the carbon shell layer on the surface of the composite material. The composite material surface carbon layer prepared by a lower phenol dosage is thinner, and the adsorption capacity of BP-1 is weaker, and it may also affect the degree of carbon thermal reduction of ferroferric oxide to zero-valent iron inside the composite material, so it shows relatively weak PS activation ability. The composite material surface carbon layer prepared by a higher phenol dosage is thicker, although its adsorption capacity for BP-1 is enhanced, but the content of zero-valent iron in the composite material is reduced, so it will also reduce its activation performance for PS.

[0137] The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials of Examples 1, 11, and 12 are as follows: Fig. 9 Formaldehyde is used to react with phenol to generate phenolic resin. Since the amount of formaldehyde is excessive, when the amount of phenol is fixed, the coating thickness of the phenolic resin on the surface of the nano-ferroferric oxide is not much different, and the thickness of the carbon layer on the surface of the composite material finally prepared does not change much. Therefore, all the composite materials in the corresponding examples show a high PS activation ability, and the degradation rate of BP-1 within 10 minutes exceeds 93%.

[0138] The degradation kinetics of BP-1 by activated PS of carbon-coated core-shell nano zero-valent iron composite materials of Examples 1, 13, and 14 are as follows: Fig.10 Since the carbon thermal reduction temperature investigated in the experiment was relatively high, ferroferric oxide could be completely reduced to zero-valent iron. Therefore, within the investigated temperature range, all composite materials showed high PS activation ability with no significant difference.

Claims

1. A method for preparing a carbon-coated nanometer zero-valent iron material with a core-shell stable structure, characterized in that: The following steps are involved: S1. Ultrasonic dispersion: Weigh 1 to 5 parts by weight of a phenolic substance and dissolve it in a mixed solution consisting of 20 parts by weight of anhydrous ethanol and 50 parts by weight of water. Then, add 1 part by weight of nano-ferroferric oxide microspheres to the mixed solution, and disperse the mixed solution under ultrasonic conditions for 10 to 15 minutes. S2, stirring reaction: adding ammonia water and 1 to 10 parts by weight of formaldehyde to the mixed solution obtained in step S1 in sequence, so that the molar concentration of ammonia in the mixed solution is 0.1 to 0.5 mol / L, then mechanically stirring the mixed solution at 30° C. for 1 hour, and then treating the mixed solution by magnetic decantation to obtain a magnetic fluid mixture, washing the magnetic fluid mixture with deionized water until neutral to obtain solid particles, and then drying the solid particles to obtain a phenolic resin-coated nano-ferrosoferric oxide composite material; S3, high-temperature calcination: placing the nano-ferroferric oxide composite material obtained in step S2 in a tube furnace, filling it with inert gas protection and calcining it at 750-950° C. for 5-6 hours to obtain a carbon-coated core-shell nano-zero-valent iron composite material; The method for treating the mixed solution by magnetic decantation in step S2 is as follows: the mixed solution is subjected to magnetic decantation treatment by a magnetic decantation component, the supernatant of the mixed solution is removed to obtain a lower layer of magnetic fluid liquid, the lower layer of magnetic fluid liquid is then mixed with deionized water at a weight ratio of 1:5, and the mixed solution is subjected to magnetic decantation treatment by the magnetic decantation component again, and the magnetic decantation treatment is repeated three times to finally obtain a magnetic fluid mixture; The magnetic decantation assembly comprises a magnetic decantation barrel (1), a base (2) located at the bottom of the magnetic decantation barrel (1), a cover plate (11) provided at the front end of the magnetic decantation barrel (1), a slot (12) provided at the cover plate (11) and the bottom of the magnetic decantation barrel (1), a sliding baffle (13) slidably connected to the slot (12) provided at the front end of the cover plate (11), a magnet (3) slidably connected to the bottom of the magnetic decantation barrel (1) provided at the bottom of the rear end of the sliding baffle (13), and a magnet (3) slidably connected to the bottom of the inner wall of the magnetic decantation barrel (1) provided at the upper part of the rear end of the sliding baffle (13). The liquid level baffle (4) is provided with a sealing plate (5) for sealing the slot (12) at the rear end of the magnet (3); the sealing plate (5) is slidably and sealedly connected to the bottom of the magnetic decantation barrel (1); a fixing block (6) is provided at the rear end of the sealing plate (5); a fixing groove (61) for accommodating the sealing plate (5) and slidably connected to the sealing plate (5) is provided at the front end of the fixing block (6); the bottom of the fixing block (6) is fixedly connected to the base (2); the top of the fixing block (6) is fixedly connected to the magnetic decantation barrel (1); and the top of the magnetic decantation barrel (1) is provided with a water inlet (14); A slide rail (7) is provided on each side of the upper surface of the base (2), and a slide groove (71) is provided on the inner wall of the slide rail (7). A slide rod (72) is provided in the slide groove (71) for sliding connection. The slide rod (72) is fixedly connected to the front end of the sealing plate (5) and is used to drive the sealing plate (5), the magnet (3) and the sliding baffle (13) to slide. A telescopic motor (73) is provided at the front end of the slide rail (7). The output end of the telescopic motor (73) is connected to the slide rod (72) for pushing the slide rod (72) to move. A drainage groove (21) is provided in the middle of the surface, and the drainage groove (21) extends from the rear end of the slot (12) to the front end of the base (2). A stirring motor (8) is provided in the middle of the rear end of the magnetic decantation barrel (1). The output end of the stirring motor (8) passes through the magnetic decantation barrel (1) and is connected to a stirring rod (81) located in the middle of the magnetic decantation barrel (1). The stirring rod (81) is provided with a plurality of groups of stirring blades (82), and the lower end of the stirring range of the stirring blades (82) is located above the liquid level baffle (4).

2. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The phenolic substance in step S1 is one or two of phenol, resorcinol, hydroquinone and phloroglucinol.

3. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The particle size of the nano-ferroferric oxide microspheres in step S1 is 20 to 100 nm.

4. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The rotation speed of the mechanical stirring in step S2 is 200-300 rpm.

5. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The method for washing the magnetic fluid mixture with deionized water to neutrality in step S2 is as follows: placing the magnetic fluid mixture in a centrifuge and centrifuging it at a speed of 3000-3500 rpm for 15-20 minutes to obtain a primary centrifuged mixture, washing the primary mixture with deionized water, and repeating the above centrifugation process three times to obtain the final solid particles.

6. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The method for drying the solid particles in step S2 is: vacuum drying the solid particles at 70-80° C. for 12 hours.

7. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: In step S3, the inert gas is argon.

8. The method for preparing a carbon-coated nano zero-valent iron material with a core-shell stable structure according to claim 1, characterized in that: The carbon-coated core-shell nano zero-valent iron composite material obtained in step S3 is applied to the advanced oxidation degradation process of organic pollutants in water using a persulfate activator.