A high-density cement slurry system with large temperature difference and wide temperate zone and its evaluation method
By using a high-density cement slurry system with a large temperature difference and a wide temperature range in deep shale gas cementing, combined with temperature and pressure increase and constant temperature and pressure hydration experiments, the problem of strong sensitivity of cement slurry thickening time under high temperature and pressure was solved, and the top strength was achieved. rapid development and improvement of construction safety.
Patent Information
- Application Number
- CN202111035544.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-09-03
AI Technical Summary
In deep shale gas cementing operations, cement slurry is highly sensitive to thickening time under high temperature and high pressure conditions, resulting in slow top strength development, and large amounts of retarder can easily lead to super-retarded setting, affecting construction safety.
It adopts a high-density cement slurry system with a large temperature difference and a wide temperature range, including oil well cement, weighting agent, high temperature resistant elastic agent, high temperature resistant water loss reducing agent, expansion agent, strength enhancer, dispersant, defoaming agent, type I retardant and retarder. Coagulant type II, the formula is optimized through temperature and pressure increase and constant temperature and pressure hydration experiments, and the temperature is lowered to the top temperature of the well for strength testing to ensure the stability and high temperature resistance of the slurry.
It achieves the rapid development of top strength under a temperature difference of 110°C, reduces the temperature sensitivity of thickening time, avoids the problem of super-retarded setting, and improves construction safety and cementing quality.
Smart Images

Figure BDA0003246073950000161 
Figure BDA0003246073950000171 
Figure FDA0004825092230000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil well cementing, and in particular relates to a high-density cement slurry system with a large temperature difference and a wide temperate zone and an evaluation method thereof. Background Art
[0002] The shale gas reservoirs in southern Sichuan are deeply buried and have high temperatures and pressures, which greatly increases the difficulty of cementing. Not only does the site need to ensure stable annular pressure, but the cement slurry also needs to be resistant to high temperatures and to rapidly develop the strength of the cement stone top under large temperature difference conditions.
[0003] In the process of deep shale gas cementing, in order to ensure that the cement slurry has enough pumping time under high temperature and high pressure conditions, the amount of retarder is greatly increased, resulting in the problem of super-retardation of the top cement slurry. In particular, the lower the top temperature, the more difficult it is for the cement stone to develop strength under the same temperature difference. In order to improve the strength development of the top of the cement stone, the method of adding early strength agent is usually adopted. However, the addition of early strength agent can easily affect the thickening time of cement slurry at high temperature, which is difficult to control on site. The cement slurry has a strong sensitivity to thickening temperature in the temperature range above 130°C. A slight increase in the bottom hole temperature will lead to a significant reduction in the thickening time, which seriously affects the safety of cementing construction on site. Summary of the invention
[0004] In view of this, the purpose of the present invention is to overcome the problems existing in the prior art and provide a high-density cement slurry system with a large temperature difference and a wide temperate zone, which can avoid the problem of slow strength development of the high-density cement slurry system in the top low-temperature section after passing through the bottom of the well, and has lower temperature sensitivity in the high-temperature section, thereby reducing the risk of on-site construction.
[0005] The present invention provides a high-density cement slurry system with a large temperature difference and a wide temperate zone, which comprises, by weight:
[0006] 100 parts of oil well cement;
[0007] 80-100 parts of weighting agent;
[0008] 2 to 6 parts of high temperature resistant elastic agent;
[0009] 1.5-2.5 parts of high temperature resistant fluid loss reducer;
[0010] 1 to 1.5 parts of expansion agent;
[0011] 1 to 5 parts of strength enhancer;
[0012] Dispersant 0.5-1 part;
[0013] Defoaming agent 0.2-0.3 parts;
[0014] 4 to 8 parts of retarder type I; the retarder type I is a multi-polymer of acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and acrylamide;
[0015] 1-2 parts of retarder II type; the retarder II type is a multi-polymer of dicarboxyl monomer, acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid;
[0016] 50-55 parts of water.
[0017] Preferably, the oil well cement is oil well G grade cement.
[0018] Preferably, the weighting agent is selected from one or more of iron powder and hematite.
[0019] Preferably, the high temperature resistant elastic agent is selected from one or more of high temperature resistant modified polyester thermoplastic materials and high temperature resistant modified fluororubber powder.
[0020] Preferably, the high temperature resistant fluid loss reducer is obtained by polymerizing substances including AMPS, low molecular weight amides and polyhydroxy carboxylic acids.
[0021] Preferably, the expansion agent includes one or more of aluminum powder, calcium oxide and magnesium oxide.
[0022] Preferably, the strength enhancer is latex.
[0023] Preferably, the dispersant is formaldehyde acetone condensate.
[0024] Preferably, the defoaming agent is one or more of a polyether defoaming agent or a silicone defoaming agent.
[0025] Preferably, the water is fresh water.
[0026] The present invention provides an evaluation method for a high-density cement slurry system with a large temperature difference and a wide temperature zone as described in the above technical solution, comprising:
[0027] According to the bottom hole temperature and pressure, the high-density cement slurry system with large temperature difference and wide temperate zone is subjected to temperature and pressure increase and constant temperature and pressure hydration experiments;
[0028] When the hydration experiment time reaches the end time node of the on-site construction slurry replacement, the temperature is lowered to the well top temperature, the slurry is taken out for strength maintenance, and a strength test is carried out after 72 hours.
[0029] The high-density cement slurry system with a large temperature difference and a wide temperature zone provided by the present invention can form a system that can meet the top strength development demand of a temperature difference of 110°C, and the lowest top temperature reaches 25°C; the system has a wide temperature zone, and under the same retarder dosage, the thickening time at 130-160°C varies little; the cement slurry system formed by compounding two retarders can solve the problem of super-retarded setting of the top cement slurry, and the top strength development is not inverted; the system has low temperature sensitivity, which solves the problem that the thickening time of the cement slurry is sharply shortened at high temperatures, affecting construction safety.
[0030] The large temperature difference, wide temperate zone, high-density cement slurry system provided by the present invention has good slurry stability, strong high temperature resistance, low temperature sensitivity under high temperature conditions, and rapid strength development of the cement stone top under large temperature differences without inversion, which can meet the deep shale gas cementing needs and improve the cementing quality. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other examples improved or modified by ordinary technicians in this field belong to the scope of protection of the present invention. It should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention. In the embodiments, the methods used are conventional methods unless otherwise specified.
[0032] The present invention provides a high-density cement slurry system with a large temperature difference and a wide temperate zone, which comprises, by weight:
[0033] 100 parts of oil well cement;
[0034] 80-100 parts of weighting agent;
[0035] 2 to 6 parts of high temperature resistant elastic agent;
[0036] 1.5-2.5 parts of high temperature resistant fluid loss reducer;
[0037] 1 to 1.5 parts of expansion agent;
[0038] 1 to 5 parts of strength enhancer;
[0039] Dispersant 0.5-1 part;
[0040] Defoaming agent 0.2-0.3 parts;
[0041] 4 to 8 parts of retarder type I; the retarder type I is a multi-polymer of acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid and acrylamide;
[0042] 1-2 parts of retarder II type; the retarder II type is a multi-polymer of dicarboxyl monomer, acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid;
[0043] 50-55 parts of water.
[0044] In the present invention, the oil well cement is preferably oil well G grade cement, more preferably oil well G grade cement that complies with API specifications and can be purchased from the market.
[0045] In the present invention, the weight proportion of the weighting agent is preferably 85 to 95 parts, more preferably 88 to 92 parts, and most preferably 90 parts.
[0046] In the present invention, the weighting agent is preferably one or more of iron powder and hematite, more preferably rhombic or rhombic iron powder; or reduced iron powder. In the present invention, the density of the rhombic iron powder is preferably 5.0-7.0 g / cm 3 , more preferably 5.5 to 6.5 g / cm 3 , most preferably 6g / cm 3 In the present invention, the particle size of the weighting agent is preferably 120-300 mesh, more preferably 150-250 mesh, more preferably 180-220 mesh, and most preferably 200 mesh. In the present invention, the weighting agent is preferably designed to be a rhombus or rhombus-like shape, which can improve the bite ability of the weighting agent and the cement matrix on the basis of improving the fluidity of the slurry and increase the strength of the high-density cement stone.
[0047] In the present invention, the weight proportion of the high temperature resistant elastic agent is preferably 3 to 5 parts, more preferably 4 parts.
[0048] In the present invention, the high temperature resistant elastic agent is preferably selected from one or more of high temperature resistant modified polyester thermoplastic materials and high temperature resistant modified fluororubber powders, and more preferably selected from one or more of surface modified high temperature resistant modified polyester thermoplastic materials and high temperature resistant modified fluororubber powders. In the present invention, the particle size of the high temperature resistant elastic agent is preferably 90 to 200 meshes, more preferably 100 to 180 meshes, more preferably 120 to 160 meshes, more preferably 130 to 150 meshes, and most preferably 140 meshes.
[0049] In the present invention, the high temperature resistant elastic agent is preferably a high temperature resistant modified polyester thermoplastic material. In the present invention, the preparation method of the high temperature resistant modified polyester thermoplastic material preferably comprises:
[0050] Mixing KH570 (silane coupling agent) and TPEE (thermoplastic polyester elastomer) to obtain a first solution;
[0051] Mixing 2-acrylamido-2-methylpropanesulfonic acid, water, potassium hydroxide, azobisisobutyronitrile and potassium persulfate to obtain a second solution;
[0052] The first solution and the second solution are mixed to obtain a high temperature resistant modified polyester thermoplastic material.
[0053] In the present invention, the mixing temperature of KH570 and TPEE is preferably 80-120° C., more preferably 90-110° C., and most preferably 100° C.; the mixing time is preferably 20-40 min, more preferably 25-35 min, and most preferably 30 min.
[0054] In the present invention, the mixing temperature of the first solution and the second solution is preferably 70-90°C, more preferably 75-85°C, most preferably 80°C; the mixing time is preferably 25-35 min, more preferably 28-32 min, most preferably 30 min.
[0055] In the present invention, the mass ratio of KH570, TPEE, 2-acrylamido-2-methylpropanesulfonic acid, water, potassium hydroxide, azobisisobutyronitrile and potassium persulfate is preferably 100: (80-120): (25-35): (55-65): (6-10): (0.3-0.7): (0.4-0.8), more preferably 100: (90-110): (28-32): (58-62): (7-9): (0.4-0.6): (0.5-0.7), and most preferably 100: 100: 30: 60: 8: 0.5: 0.6.
[0056] In the present invention, the first solution and the second solution after mixing preferably further comprise:
[0057] The obtained mixed product is crushed and granulated to obtain a high temperature resistant modified polyester thermoplastic material.
[0058] In the present invention, the high temperature resistant elastic agent can be adsorbed or evenly dispersed between cement particles, has strong high temperature resistance, and increases the deformability of cement stone at higher temperatures.
[0059] In the present invention, the weight proportion of the high temperature resistant fluid loss reducer is preferably 1.8 to 2.2 parts, more preferably 2 parts.
[0060] In the present invention, the high temperature resistant fluid loss reducer is preferably obtained by polymerization modification of materials including AMPS, low molecular weight amide and polyhydroxy carboxylic acid, and can be purchased from the market.
[0061] In the present invention, the weight proportion of the expansion agent is preferably 1.1 to 1.4 parts, more preferably 1.2 to 1.3 parts.
[0062] In the present invention, the expansion agent preferably includes one or more of aluminum powder, calcium oxide and magnesium oxide. In the present invention, the expansion agent can compensate for the shrinkage of high-density cement paste.
[0063] In the present invention, the weight proportion of the strength enhancer is preferably 2 to 4 parts, more preferably 3 parts.
[0064] In the present invention, the strength enhancer is preferably latex, which can be solid latex powder or liquid latex; the weight proportion of the solid latex powder is preferably 1 to 2 parts, more preferably 1.2 to 1.8 parts, and most preferably 1.4 to 1.6 parts; the weight proportion of the liquid latex is preferably 3 to 5 parts, more preferably 3.5 to 4.5 parts, and most preferably 3 parts.
[0065] In the present invention, the strength enhancer can improve the bonding strength between the admixture and the cement matrix, thereby improving the strength of the cement paste.
[0066] In the present invention, the weight proportion of the dispersant is preferably 0.5 to 1 part, more preferably 0.6 to 0.9 part, and most preferably 0.7 to 0.8 part.
[0067] In the present invention, the dispersant is preferably a formaldehyde acetone condensate.
[0068] In the present invention, the weight portion of the defoaming agent is preferably 0.25 parts.
[0069] In the present invention, the defoaming agent is preferably selected from one or more of polyether defoaming agents or silicone defoaming agents.
[0070] In the present invention, the weight proportion of the retarder type I is preferably 5 to 7 parts, more preferably 6 parts.
[0071] In the present invention, the preparation method of the retarder type I preferably comprises:
[0072] Under the action of an initiator, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid and a molecular weight regulator are first reacted to obtain a retarder type I.
[0073] In the present invention, in the first reaction process, acrylamide and 2-acrylamide-2-methylpropanesulfonic acid are preferably dissolved in water to adjust the pH value, and then acrylic acid, a molecular weight regulator and an initiator are added to carry out the first reaction.
[0074] In the present invention, the water is preferably distilled water.
[0075] In the present invention, NaOH solution is preferably used in the pH adjustment process; the pH is preferably adjusted to 8-9, more preferably 8.5.
[0076] In the present invention, the initiator is preferably NaHSO3.
[0077] In the present invention, the molecular weight regulator is preferably a MgCl2 solution.
[0078] In the present invention, the mass ratio of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, molecular weight regulator and initiator is preferably (620-640): (40-60): (20-30): (2-4): (1-3), more preferably (625-635): (45-55): (23-27): (2.5-3.5): (1.5-2.5), and most preferably 630: 50: 25: 3: 2.
[0079] In the present invention, the temperature of the first reaction is preferably 50-60°C, more preferably 52-58°C, more preferably 54-56°C, and most preferably 55°C; the first reaction is preferably carried out under stirring; the time of the first reaction is preferably 460-500 min, more preferably 470-490 min, and most preferably 480 min.
[0080] In the present invention, the weight proportion of the retarder type II is preferably 1.2 to 1.8 parts, more preferably 1.4 to 1.6 parts, and most preferably 1.5 parts.
[0081] In the present invention, the preparation method of the retarder type II preferably comprises:
[0082] Under the action of an initiator, a dicarboxyl monomer, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and a molecular weight regulator are subjected to a second reaction to obtain a retarder type II.
[0083] In the present invention, the initiator is consistent with the initiator described in the above technical solution, and will not be described in detail here.
[0084] In the present invention, the dicarboxyl monomer is preferably selected from itaconic acid.
[0085] In the present invention, in the second reaction process, the dicarboxyl monomer is preferably heated and dissolved in water, acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid are added and dissolved in water, and then a molecular weight regulator and an initiator are added to carry out the second reaction.
[0086] In the present invention, the mass ratio of the dicarboxyl monomer, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, molecular weight regulator and initiator is preferably (30-40):(10-20):(680-720):(1-3):(1-3), more preferably (33-37):(13-17):(690-710):(1.5-2.5):(1.5-2.5), and most preferably 35:15:700:2:2.
[0087] In the present invention, the temperature of the second reaction is preferably 55-65°C, more preferably 58-62°C, and most preferably 60°C; the second reaction is preferably carried out under stirring; the time of the second reaction is preferably 510-530 min, more preferably 515-525 min, and most preferably 520 min.
[0088] In the present invention, the preparation method of the large temperature difference wide temperature zone high density cement slurry system preferably comprises:
[0089] Oil well cement, weighting agent, high temperature elastic agent, high temperature fluid loss reducer, expansion agent, strength enhancer, dispersant, defoamer, retarder I type, retarder II type and water are mixed to obtain a high-density cement slurry system with a large temperature difference and wide temperate zone.
[0090] In the present invention, the mixing is preferably carried out under stirring conditions; the stirring speed is preferably 3500-4500 r / min, more preferably 3800-4200 r / min, and most preferably 4000 r / min.
[0091] The present invention provides an evaluation method for a high-density cement slurry system with a large temperature difference and a wide temperature zone as described in the above technical solution, comprising:
[0092] According to the bottom hole temperature and pressure, the high-density cement slurry system with large temperature difference and wide temperate zone is subjected to temperature and pressure increase and constant temperature and pressure hydration experiments;
[0093] When the hydration experiment time reaches the end time node of the on-site construction slurry replacement, the temperature is lowered to the well top temperature, the slurry is taken out for strength maintenance, and a strength test is carried out after 72 hours.
[0094] In the present invention, the bottom hole temperature is preferably the bottom hole circulation temperature.
[0095] In the present invention, the temperature rise time during the hydration experiment is preferably the time it takes for the large temperature difference, wide temperature range and high density cement slurry system to reach the bottom of the well.
[0096] In the present invention, the hydration experiment preferably includes:
[0097] The first stage is temperature and pressure increase and the second stage is constant temperature and pressure.
[0098] In the present invention, the heating temperature is preferably 100-160°C, more preferably 110-150°C, more preferably 120-140°C, and most preferably 130°C; the boosting pressure is preferably 70-110MPa, more preferably 75-105MPa, more preferably 80-100MPa, more preferably 85-95MPa, and most preferably 90MPa; the boosting time is preferably 50-70min, more preferably 55-65min, and most preferably 60min.
[0099] In the present invention, the constant temperature and pressure refers to maintaining the temperature and pressure reached by the first stage of temperature and pressure increase; the time of the constant temperature and pressure is preferably 15 to 25 minutes, more preferably 18 to 22 minutes, and most preferably 20 minutes.
[0100] In the present invention, the cooling temperature is preferably 25-90°C, more preferably 30-85°C, more preferably 35-80°C, more preferably 40-75°C, more preferably 45-70°C, more preferably 50-65°C, and most preferably 55-65°C.
[0101] In the present invention, the pressure is preferably released during the process of taking out the slurry.
[0102] In the present invention, the curing is preferably pressurized curing, and the curing is preferably carried out in a pressurized curing kettle; the curing temperature is preferably 25-90°C, more preferably 30-85°C, more preferably 35-80°C, more preferably 40-75°C, more preferably 45-70°C, more preferably 50-65°C, and most preferably 55-65°C; the curing time is preferably 65-75 hours, more preferably 68-72 hours, and most preferably 70 hours; the curing pressure is preferably 15-25MPa, more preferably 18-22MPa, and most preferably 21MPa; the curing pressure can also be normal pressure.
[0103] In the present invention, the strength testing method is preferably to use a compressive strength testing machine for strength testing. For samples with expected strength greater than 3.5 MPa, the loading rate should be 71.7 kN / min±7.2 kN / min. For samples with expected strength equal to or less than 3.5 MPa, the loading rate should be 17.9 kN / min±1.8 kN / min. The control part of the testing machine should not be adjusted during the period when the sample is under pressure until it breaks.
[0104] The high-density cement slurry system with a large temperature difference and a wide temperature zone provided by the present invention can form a system that can meet the top strength development demand of a temperature difference of 110°C, and the lowest top temperature reaches 25°C; the system has a wide temperature zone, and under the same retarder dosage, the thickening time at 130-160°C varies little; the cement slurry system formed by compounding two retarders can solve the problem of super-retarded setting of the top cement slurry, and the top strength development is not inverted; the system has low temperature sensitivity, which solves the problem that the thickening time of the cement slurry is sharply shortened at high temperatures, affecting construction safety.
[0105] The large temperature difference, wide temperate zone, high-density cement slurry system provided by the present invention has good slurry stability, strong high temperature resistance, low temperature sensitivity under high temperature conditions, and rapid strength development of the cement stone top under large temperature differences without inversion, which can meet the deep shale gas cementing needs and improve the cementing quality.
[0106] The G-grade cement used in the embodiment of the present invention is Jiahua G-grade oil well cement produced by Sichuan Jiahua Cement Plant;
[0107] The high temperature resistant elastic agent is a high temperature resistant modified polyester thermoplastic elastic material (particle size 120 mesh), and the preparation method is as follows: weigh 100 parts of KH570 and 100 parts of TPEE powder, place them in a four-necked flask with a mechanical stirrer, a thermometer, and a condenser, heat to 100°C, and stir for about 30 minutes to completely dissolve them to form a uniform solution; weigh 30 parts of 2-acrylamide-2-methylpropane sulfonic acid and 60 parts of water, place them in an open container to fully dissolve them to form a uniform aqueous solution, and use 8 parts of potassium hydroxide; add 0.5 parts of azobisisobutyronitrile and 0.6 parts of potassium persulfate respectively and mix them; mix the two solutions, maintain the temperature at 80°C, and continue stirring for 30 minutes to obtain a block product, and after crushing and granulation, obtain a modified thermoplastic elastic material.
[0108] The weighting agent is reduced iron powder (particle size 250 mesh), which is provided by Hesheng Materials Co., Ltd.
[0109] The high temperature resistant fluid loss agent is a polymer modified product of AMPS, low molecular weight amide, polyhydroxy carboxylic acid, etc., and adopts the G33S model product provided by Weihui Chemical Co., Ltd.;
[0110] The expansion agent is a G401 product provided by Weihui Chemical Co., Ltd.
[0111] The strength enhancer is a water-soluble dispersible latex powder, and the product of model WWJF-8050 provided by Changzhou Songbai Chemical Co., Ltd. is used;
[0112] The dispersant is formaldehyde acetone condensate, and the BS300 product provided by Chongqing Hongsheng Chemical Co., Ltd. is used;
[0113] The defoamer used is the XP-1 model product provided by Weihui Chemical Co., Ltd.;
[0114] Retarder type I is a multi-polymer of acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and acrylamide. The preparation method is as follows: 630 parts by weight of acrylamide and 50 parts by weight of 2-acrylamide-2-methylpropanesulfonic acid are dissolved in distilled water, the pH value is adjusted to 8-9 with a NaOH solution, 25 parts by weight of acrylic acid and 3 parts by weight of a molecular weight regulator MgCl2 monomer solution are added, the solution is placed in a water bath, 2 parts by weight of a NaHSO3 initiator is added, the reaction temperature is controlled at 55°C, and the constant stirring time is 480 minutes to obtain a liquid retarder product.
[0115] Retarder II type is a multi-polymer of a dicarboxyl monomer, acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid. The preparation method is as follows: 35 parts by weight of dicarboxyl monomer itaconic acid is weighed and heated to dissolve in water, 15 parts by weight of acrylic acid and 700 parts of 2-acrylamide-2-methylpropanesulfonic acid are weighed and dissolved in water, 2 parts by weight of a molecular weight regulator MgCl2 monomer solution and 2 parts by weight of a NaHSO3 initiator are added, the reaction temperature is controlled at 60°C, and the constant stirring time is 520 minutes to obtain a retarder liquid product.
[0116] Example 1
[0117] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 20g of high temperature elastic agent (120 mesh), 8g of high temperature fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 16g of retarder I type, 4g of retarder II type, 0.8g of defoaming agent, and 220g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0118] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 1 of the present invention was evaluated:
[0119] Density test: Use a drilling fluid densitometer in accordance with the method specified in GB / T 16783.1. After the cement slurry is poured into the cup of the drilling fluid densitometer, stir it 25 times to eliminate the entrained air before measuring.
[0120] Stability test: According to the method specified in GBT 19139-2012, after stirring the cement slurry, pour the cement slurry into the sedimentation tube, stir to remove bubbles, and then place it in a heating container with water, set the temperature to 130℃, 21MPa, and after curing and solidification, cool it out, cut it into two parts, and measure the relative density.
[0121] Rheological test: According to the method specified in GBT 19139-2012, a rotational viscometer is used to read the readings at 6 speeds in ascending order and then in descending order, and the average value of the readings at each speed is calculated.
[0122] Cement slurry thickening time test: According to the method specified in GBT 19139-2012, the temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage, with the target temperature set at 130°C, the target pressure set at 80MPa, and the temperature and pressure increase time set at 60min. The second stage is the constant temperature and pressure stage, with the temperature always maintained at 130°C and the pressure at 80MPa until the slurry consistency reaches 100BC and the experiment is stopped.
[0123] Water loss test: According to the method specified in GBT 19139-2012, the cement slurry is first stirred and cured in a thickener and then tested using a static filter loss tester.
[0124] Top strength test: The slurry prepared in Example 1 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 minutes, and the target temperature was 130°C and 80 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were maintained at a constant temperature and pressure for 20 minutes; the third stage, after 20 minutes, the slurry was cooled to the top curing temperature of 80°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a pressurized curing kettle for pressurized curing. The curing conditions were 80°C, 21 MPa, and the strength was tested after 72 hours, with a loading rate of 71.7 kN / min±7.2 kN / min (a compressive strength testing machine was used for strength testing); the experimental results are shown in Tables 1 and 2.
[0125] Example 2
[0126] The same formula as in Example 1 was used. 400 g of Jiahua cement, 320 g of weighting agent (250 mesh), 20 g of high temperature elastic agent (120 mesh), 8 g of high temperature fluid loss reducer, 4 g of expansion agent, 8 g of strength enhancer, 2 g of dispersant, 16 g of retarder I type, 4 g of retarder II type, 0.8 g of defoaming agent, and 220 g of water were weighed. The above materials were mixed and stirred evenly at a speed of 4000 r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0127] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 2 of the present invention was evaluated:
[0128] Top strength test: The slurry prepared in Example 2 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 130°C and 80 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the slurry was cooled to the top curing temperature of 40°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a pressurized curing kettle for pressurized curing: curing conditions: 40°C, normal pressure, the strength was tested after 72 hours, and the loading rate was 71.7 kN / min±7.2 kN / min; the experimental results are shown in Table 2.
[0129] Example 3
[0130] The same formula as in Example 1 was used. 400 g of Jiahua cement, 320 g of weighting agent (250 mesh), 20 g of high temperature elastic agent (120 mesh), 8 g of high temperature fluid loss reducer, 4 g of expansion agent, 8 g of strength enhancer, 2 g of dispersant, 16 g of retarder I type, 4 g of retarder II type, 0.8 g of defoaming agent, and 220 g of water were weighed. The above materials were mixed and stirred evenly at a speed of 4000 r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0131] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 3 of the present invention was evaluated:
[0132] Top strength test: The slurry prepared in Example 3 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 130°C and 80 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the temperature was lowered to the top curing temperature of 25°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a normal pressure curing kettle for normal pressure curing. The curing conditions were 25°C and normal pressure. The strength was tested after 72 hours, and the loading rate was 71.7 kN / min±7.2 kN / min. The experimental results are shown in Table 2.
[0133] Example 4
[0134] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 20g of high temperature elastic agent (120 mesh), 8g of high temperature fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 24g of retarder I type, 6g of retarder II type, 0.8g of defoaming agent, and 210g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system with a large temperature difference and wide temperate zone for deep shale gas.
[0135] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 4 of the present invention was evaluated:
[0136] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130℃, the target pressure is set to 110MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130℃ and the pressure is 110MPa until the slurry consistency reaches 100BC and the experiment is stopped.
[0137] Top strength test: The slurry prepared in Example 4 was subjected to a hydration experiment on a thickening instrument. The experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 130°C and 110 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the slurry was cooled to the top curing temperature of 25°C and then taken out to remove the floating oil on the surface of the slurry, poured into a curing mold, and placed in a normal pressure curing kettle for curing. The curing conditions were 25°C and normal pressure. The strength was tested after 72 hours. The experimental results are shown in Table 2.
[0138] Example 5
[0139] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 20g of high temperature elastic agent (120 mesh), 10g of high temperature fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 24g of retarder I type, 6g of retarder II type, 0.8g of defoaming agent, and 210g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0140] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 5 of the present invention was evaluated:
[0141] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 140℃, the target pressure is set to 110MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 140℃ and the pressure is 110MPa until the slurry consistency reaches 100BC and the experiment is stopped.
[0142] Top strength test: The slurry prepared in Example 5 was subjected to a hydration experiment on a thickening instrument. The experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 140°C and 110 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the temperature was lowered to the top curing temperature of 40°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a normal pressure curing kettle for curing. The curing conditions were 40°C and normal pressure. The strength was tested after 72 hours. The experimental results are shown in Table 2.
[0143] Example 6
[0144] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 20g of high temperature elastic agent (120 mesh), 10g of high temperature fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 24g of retarder I type, 6g of retarder II type, 0.8g of defoaming agent, and 210g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0145] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 6 of the present invention was evaluated:
[0146] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 150℃, the target pressure is set to 110MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 150℃ and the pressure is 110MPa until the slurry consistency reaches 100BC and the experiment is stopped.
[0147] Top strength test: The slurry prepared in Example 6 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 150°C and 110 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the temperature was lowered to the top curing temperature of 50°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a normal pressure curing kettle for curing. The curing conditions were 50°C, normal pressure, and the strength was tested after 72 hours, with a loading rate of 71.7 kN / min±7.2 kN / min. The experimental results are shown in Table 2.
[0148] Example 7
[0149] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 20g of high temperature elastic agent (120 mesh), 10g of high temperature fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 24g of retarder I type, 6g of retarder II type, 0.8g of defoaming agent, and 210g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system with a large temperature difference and a wide temperate zone for deep shale gas.
[0150] The high-density cement slurry system with large temperature difference and wide temperate zone for deep shale gas prepared in Example 7 of the present invention was evaluated:
[0151] Density test: Use a drilling fluid densitometer in accordance with the method specified in GB / T 16783.1. After the cement slurry is poured into the cup of the drilling fluid densitometer, stir it 25 times to eliminate the entrained air before measuring.
[0152] Stability test: According to the method specified in GBT 19139-2012, after stirring the cement slurry, pour the cement slurry into the sedimentation tube, stir to remove bubbles, and then place it in a heating container with water. Set the temperature to 160℃, 21MPa. After curing and solidification, cool it down, take it out, cut it into two parts, and measure the relative density.
[0153] Rheological test: According to the method specified in GBT 19139-2012, a rotational viscometer is used to read the readings at 6 speeds in ascending order and then in descending order, and the average value of the readings at each speed is calculated.
[0154] Cement slurry thickening time test: According to the method specified in GBT 19139-2012, the temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage, with the target temperature set at 160°C and the target pressure set at 110MPa. The temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage, with the temperature maintained at 160°C and the pressure maintained at 110MPa until the slurry consistency reaches 100BC and the experiment is stopped.
[0155] Water loss test: According to the method specified in GBT 19139-2012, the cement slurry is first stirred and cured in a thickener and then tested using a static filter loss tester.
[0156] Top strength test: The slurry prepared in Example 7 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 min, and the target temperature was 160°C and 110 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 min; the third stage, after 20 min, the temperature was lowered to the top curing temperature of 50°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a normal pressure curing kettle for curing. The curing conditions were 50°C, normal pressure, and the strength was tested after 72 hours, with a loading rate of 71.7 kN / min±7.2 kN / min. The experimental results are shown in Tables 1 and 2.
[0157] Comparative Example 1
[0158] Weigh 400g of Jiahua cement, 320g of weighting agent (250 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 20g of retarder type I, 0.8g of defoaming agent, and 224g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0159] The high-density cement slurry system prepared in Comparative Example 1 of the present invention was evaluated:
[0160] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0161] Comparative Example 2
[0162] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 16g of retarder type I, 0.8g of defoaming agent, and 224g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0163] The high-density cement slurry system prepared in Comparative Example 2 of the present invention was evaluated:
[0164] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0165] Comparative Example 3
[0166] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 32g of retarder type I, 0.8g of defoaming agent, and 212g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0167] The high-density cement slurry system prepared in Comparative Example 3 of the present invention was evaluated:
[0168] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0169] Comparative Example 4
[0170] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 4g of retarder type II, 0.8g of defoaming agent, and 240g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0171] The high-density cement slurry system prepared in Comparative Example 4 of the present invention was evaluated:
[0172] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0173] Comparative Example 5
[0174] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 8g of retarder II type, 0.8g of defoaming agent, and 236g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0175] The high-density cement slurry system prepared in Comparative Example 5 of the present invention was evaluated:
[0176] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0177] Comparative Example 6
[0178] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 10g of retarder II type, 0.8g of defoaming agent, and 232g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0179] The high-density cement slurry system prepared in Comparative Example 6 of the present invention was evaluated:
[0180] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 130°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 130°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0181] Comparative Example 7
[0182] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 12g of retarder II type, 0.8g of defoaming agent, and 232g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0183] The high-density cement slurry system prepared in Comparative Example 7 of the present invention was evaluated:
[0184] The slurry prepared in Comparative Example 7 was subjected to a hydration experiment on a thickening instrument, and the experimental conditions were as follows: the first stage temperature and pressure increase time was 60 minutes, and the target temperature was 130°C and 80 MPa; the second stage, after reaching the target temperature and pressure, the temperature and pressure were kept constant for 20 minutes; the third stage, after 20 minutes, the temperature was lowered to the top curing temperature of 80°C and then taken out, the floating oil on the surface of the slurry was removed, and the slurry was poured into a curing mold and placed in a pressurized curing kettle for pressurized curing. The curing conditions were 80°C, 21 MPa, and the strength was tested after 72 hours, with a loading rate of 71.7 kN / min±7.2 kN / min. The experimental results are shown in Table 2.
[0185] Comparative Example 8
[0186] Weigh 400g of Jiahua cement, 320g of weighting agent (200 mesh), 16g of high temperature resistant elastic agent (120 mesh), 8g of high temperature resistant fluid loss reducer, 4g of expansion agent, 8g of strength enhancer, 2g of dispersant, 12g of retarder II type, 0.8g of defoaming agent, and 232g of water; mix and stir the above materials at a speed of 4000r / min to obtain a high-density cement slurry system.
[0187] The high-density cement slurry system prepared in Comparative Example 8 of the present invention was evaluated:
[0188] Cement slurry thickening time test: The temperature and pressure of the thickener are set to two stages. The first stage is the temperature and pressure increase stage. The target temperature is set to 135°C, the target pressure is set to 80MPa, and the temperature and pressure increase time is 60min. The second stage is the constant temperature and pressure stage. The temperature is always maintained at 135°C and the pressure is 80MPa until the slurry consistency reaches 100BC and the experiment is stopped. The experimental results are shown in Table 2.
[0189] Table 1 Performance test results of products prepared in the embodiments of the present invention and comparative examples
[0190]
[0191] Table 2 Evaluation results of products prepared in the examples of the present invention and the comparative examples
[0192]
[0193] As can be seen from Table 1, in Comparative Examples 1 to 3, retarder type I is used alone, and the amount of retarder added is large, and the effect of extending the thickening time is limited; in Comparative Examples 4 to 8, retarder type II is used alone. When the amount added exceeds 3%, the cement slurry in the top low-temperature section is super-retarded, and the strength of the cement stone develops slowly, affecting the sealing quality. In addition, at high temperatures, the thickening time is greatly reduced, and the temperature sensitivity is strong, which affects the construction safety on site. In Examples 1 to 7, the cement slurry system formed by compounding two retarders in proportion has low temperature sensitivity under high temperature conditions at the bottom of the well. In the range of 130 to 160°C, the difference in thickening time under the same amount of retarder is not large, which is conducive to slowing down the impact of bottom temperature changes on construction time and reducing construction risks; the top strength develops quickly under large temperature differences, without inversion, and the top strength development under a maximum temperature difference of 110°C can be achieved, and the lowest temperature at the top reaches 25°C, which is conducive to ensuring the sealing requirements of deep wells and long sealing.
[0194] The high-density cement slurry system with a large temperature difference and a wide temperature zone provided by the present invention can form a system that can meet the top strength development demand of a temperature difference of 110°C, and the lowest top temperature reaches 25°C; the system has a wide temperature zone, and under the same retarder dosage, the thickening time at 130-160°C varies little; the cement slurry system formed by compounding two retarders can solve the problem of super-retarded setting of the top cement slurry, and the top strength development is not inverted; the system has low temperature sensitivity, which solves the problem that the thickening time of the cement slurry is sharply shortened at high temperatures, affecting construction safety.
[0195] The large temperature difference, wide temperate zone, high-density cement slurry system of the present invention has good slurry stability, strong high temperature resistance, low temperature sensitivity under high temperature conditions, fast strength development of cement stone top under large temperature difference, and no inversion, which can meet the deep shale gas cementing needs and improve cementing quality.
[0196] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A high-density cement slurry system with a large temperature difference and a wide temperate zone, comprising, by weight: The retarder type I is a multi-polymer of acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and acrylamide; the preparation method of the retarder type I comprises: under the action of an initiator, acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid and a molecular weight regulator are subjected to a first reaction to obtain retarder type I; wherein the mass ratio of acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, acrylic acid, molecular weight regulator and initiator is (620-640): (40-60): (20-30): (2-4): (1-3); The retarder type II is a multi-polymer of a dicarboxyl monomer, acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid; the preparation method of the retarder type II comprises: under the action of an initiator, the dicarboxyl monomer, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and a molecular weight regulator are subjected to a second reaction to obtain a retarder type II; wherein the mass ratio of the dicarboxyl monomer, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, the molecular weight regulator and the initiator is (30-40): (10-20): (680-720): (1-3): (1-3).
2. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The oil well cement is oil well G grade cement.
3. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The weighting agent is selected from one or more of iron powder and hematite.
4. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The high temperature resistant elastic agent is selected from one or more of high temperature resistant modified polyester thermoplastic material and high temperature resistant modified fluororubber powder.
5. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The high temperature resistant fluid loss reducer is obtained by polymerizing substances including AMPS, low molecular weight amide and polyhydroxy carboxylic acid.
6. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The expansion agent includes one or more of aluminum powder, calcium oxide and magnesium oxide.
7. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The strength enhancer is latex.
8. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The dispersant is formaldehyde acetone condensate.
9. The high-density cement slurry system with large temperature difference and wide temperate zone according to claim 1, characterized in that: The defoamer is selected from one or more of polyether defoamers or silicone defoamers.
10. An evaluation method for a high-density cement slurry system with a large temperature difference and a wide temperature range according to claim 1, comprising: According to the bottom hole temperature and pressure, the high-density cement slurry system with large temperature difference and wide temperate zone is subjected to temperature and pressure increase and constant temperature and pressure hydration experiments; When the hydration experiment time reaches the end time node of the on-site construction slurry replacement, the temperature is lowered to the well top temperature, the slurry is taken out for strength maintenance, and a strength test is carried out after 72 hours.
Citation Information
Patent Citations
Upside-down-hanging-preventing wide-temperate-zone oil well cement retarder
CN103013481A
Medium-high-temperature oil well cement retarding agent as well as preparation method and application thereof
CN109503760A
Oil well cement paste system for preventing high-temperature strength retrogression and preparation method thereof
CN110484223A
Cement paste system and preparation method thereof
CN112299757A
High-temperature-resistant large-temperature-difference elastic-tough cement paste system and preparation method thereof
CN112479635A