A kind of imitation electroplating aluminum paste and preparation method thereof
By grinding and kneading spherical aluminum powder, linoleic acid, isostearic acid and decayl polyoxyethylene ether monoacid, combined with dilution and coupling agent treatment, the existing aluminum paste in terms of color, appearance and dispersion are solved. Problem, the preparation of imitation electroplating aluminum paste is achieved with brighter, more delicate, high coverage and good dispersion.
Patent Information
- Application Number
- CN202211430026.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-15
AI Technical Summary
The existing imitation electroplating aluminum paste has shortcomings in color, paint film appearance, water surface coverage and storage dispersion. The white brightness is insufficient, the gloss is not fine enough, the water surface coverage is not complete, and the aluminum sheets are prone to agglomeration after a long storage time, resulting in degradation of dispersion performance. .
Grinding and kneading using spherical aluminum powder, grinding solvent, linoleic acid, isostearic acid and decayl polyoxyethylene ether monoacid. The aluminum slurry filter cake was obtained by sieving and filtration, and dilution solvent was added and coupling was added. to ensure the dispersion and compatibility of aluminum paste.
It improves the white brightness of aluminum paste, the delicate appearance of the paint film, the water surface coverage and storage dispersion, ensures that the product has good dispersion performance during the storage period, and is suitable for a variety of coating systems.
Smart Images

Figure CN115780797B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum paste preparation, and in particular to an imitation electroplating aluminum paste and a preparation method thereof. Background Art
[0002] Aluminum paste (aluminum paste for short), also known as aluminum pigment or aluminum silver paste, is a decorative metal pigment that must be used in coatings or inks. The main components of aluminum paste are flaky and silver-circular aluminum particles and mineral oil solvents; the aluminum paste is paste-like in form; the characteristics of aluminum paste are smooth and flat aluminum flakes, concentrated particle size distribution with a small span, regular shape, excellent light reflection performance and metallic effect, and the paint film after mixing with transparent color pigments presents excellent angle-dependent color effects. Aluminum paste is mainly used in automotive coatings, 3C coatings, toy paints, industrial paints, food packaging and cosmetics.
[0003] In recent years, aluminum paste products produced in the industry have begun to develop in the direction of fine-particle aluminum paste, but there is still room for improvement in terms of color, film appearance, water surface coverage and storage dispersibility. Specifically, the current market imitation electroplating aluminum paste has poor white brightness in terms of color; in terms of film appearance, the luster is astringent and not delicate enough; in terms of water surface coverage, it is easy to have incomplete coverage; in terms of storage dispersibility, if the aluminum paste is stored for a longer time (more than 6 months), the oleic acid is oxidized into epoxy oleate by the moisture in the air or solvent, making the aluminum flakes in the aluminum paste easy to agglomerate and difficult to disperse, greatly reducing the dispersion performance of the aluminum paste.
[0004] In view of the above color performance defects, some enterprises do not use oleic acid, but use stearic acid, which improves the whiteness of the imitation electroplating aluminum paste, but its brightness decreases. In addition, because oleic acid is easily oxidized with moisture in the air or solvent to form epoxy oleic acid, the organic solvent used for grinding is easy to turn black, which greatly reduces the number of organic solvent recycling. In addition, stearic acid is only suitable for making floating aluminum paste, not for making non-floating aluminum paste. Because the fatty acid in stearic acid is too saturated, the aluminum paste floats on the surface layer of the paint film after being made into a paint film, and it is easy to produce silver throwing after construction and drying.
[0005] In summary, it is very important to provide an electroplating aluminum paste with a brighter white color, a fine and silky paint film appearance, a strong water surface coverage and good storage dispersibility and a preparation method thereof. Summary of the invention
[0006] The object of the present invention is to provide an imitation electroplating aluminum paste and a preparation method thereof, and the specific technical scheme is as follows:
[0007] In a first aspect, the present invention provides a method for preparing an electroplating aluminum paste, comprising the following steps:
[0008] Step S1, adding spherical aluminum powder, grinding solvent, linoleic acid, isostearic acid and decanol polyoxyethylene ether monoester into a ball mill and grinding;
[0009] Step S2, grinding, screening and filter pressing to prepare aluminum slurry filter cake;
[0010] Step S3, adding a diluting solvent and a coupling agent to the aluminum paste filter cake, stirring and adding the mixture to a kneader for kneading to obtain a product imitating electroplating aluminum paste.
[0011] Optionally, in step S1 and step S3, the mass ratio of the spherical aluminum powder, grinding solvent, linoleic acid, isostearic acid, decanol polyoxyethylene ether monoester, dilution solvent and coupling agent is (75-85): (155-165): (1.5-2): (1-4.0): (1-2): (15-18): (0.7-1.2).
[0012] Optionally, in step S1, the spherical aluminum powder has a D50 of 1-3 μm.
[0013] Optionally, the grinding solvent used in step S1 includes 150# solvent oil and D70 solvent oil, and the mass ratio of the 150# solvent oil to the D70 solvent oil is 4:1 to 1:1;
[0014] In step S3, the dilution solvent includes D40 solvent oil; and the coupling agent includes isopropyl triisostearyl titanate.
[0015] Optionally, the medium used for grinding in step S1 is a plurality of bearing steel balls with a diameter of 0.6 mm to 1.0 mm.
[0016] Optionally, the grinding time in step S1 is 35 to 45 hours.
[0017] Optionally, in step S1, the rotation speed of the ball mill is 45 r / min.
[0018] Optionally, during grinding in step S1, the outer wall temperature of the ball mill does not exceed 50°C.
[0019] Optionally, the kneading time used in step S3 is 30 minutes.
[0020] In a second aspect, the present invention provides an imitation electroplating aluminum paste prepared by the method for preparing the imitation electroplating aluminum paste, wherein the imitation electroplating aluminum paste comprises the following components in percentage by mass:
[0021] The content of aluminum flakes is 63% to 67%, grinding solvent is 19%, dilution solvent is 15%, isostearic acid is 0.2% to 0.5%, decanol polyoxyethylene ether monoester is 0.1% to 0.3% and linoleic acid is 0.4%.
[0022] The application of the technical solution of the present invention has the following beneficial effects:
[0023] In the preparation method of the electroplating aluminum paste described in the present invention, when grinding the spherical aluminum powder in step S1, a grinding agent is used to help wet and disperse the spherical aluminum powder; isostearic acid and linoleic acid are used to lubricate and protect the ground spherical aluminum powder, ensuring that the spherical aluminum powder is ground very thinly, very flatly and not broken, so that the appearance of the paint film of the product is as delicate as silk; at the same time, isostearic acid and linoleic acid are used to help grind off the thin layer of aluminum oxide on the surface of the spherical aluminum powder during grinding, revealing the silver-white color of the aluminum flakes, thereby improving the white brightness of the product; subsequently, the silver-white aluminum flakes are wrapped and protected by decanol polyoxyethylene ether monoester, linoleic acid, isostearic acid and grinding solvent, and the decanol polyoxyethylene ether monoester with hydrophilic and lipophilic groups can effectively isolate the moisture in the air and the grinding solvent, avoiding the oxidation of isostearic acid, linoleic acid and the ground aluminum flakes by oxygen in the moisture, thereby preventing the aluminum flakes from agglomerating during the storage period, and ensuring that the product has good dispersibility and a strong water surface coverage rate;
[0024] In step S2, screening and filter pressing ensure the purity and uniformity of the aluminum slurry particle size, and further ensure that the product's paint film appearance is as fine as silk;
[0025] In step S3, adding a dilution solvent facilitates adjusting the aluminum content in the product, and adding a coupling agent facilitates improving the compatibility with downstream coating systems (such as acrylic resin systems, epoxy resin systems, hydroxyl resin systems, and polyurethane resin systems) and improving the wear resistance of the coating film. The combined use of steps S1 to S3 of the present invention can ensure that the prepared product has a whiter color, a fine and silky appearance of the paint film, a strong water surface coverage, and good storage dispersibility.
[0026] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0028] Figure 1 This is an electron microscope micrograph of the aluminum paste product in Example 1 of the present invention;
[0029] Figure 2 This is an electron microscope micrograph of the aluminum paste product in Comparative Example 1;
[0030] Figure 3 This is an electron microscope micrograph of the aluminum paste product in Comparative Example 2;
[0031] Figure 4 This is an electron microscope micrograph of the aluminum paste product in Comparative Example 3;
[0032] Figure 5 This is an electron microscope micrograph of the aluminum paste product in Comparative Example 4. DETAILED DESCRIPTION
[0033] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] A method for preparing an electroplating aluminum paste comprises the following steps:
[0036] Step S1, adding 80 kg of spherical aluminum powder, 160 kg of grinding solvent, 1.5 kg of linoleic acid, 1 kg of isostearic acid and 1 kg of decanol polyoxyethylene ether monoester into a ball mill (specifically a horizontal ball mill with a diameter of 900 mm and a length of 1500 mm) for grinding;
[0037] Step S2, after grinding, sieving ((passing through a 500-mesh screen)), and filter pressing to prepare an aluminum slurry filter cake with a solid content of 75±2%, about 100 kg;
[0038] Step S3, adding 15 kg of dilution solvent and 0.7 kg of coupling agent to the aluminum paste filter cake, stirring evenly, adding to a kneader and kneading to obtain about 115.7 kg of imitation electroplating aluminum paste, wherein the aluminum content is 65±2%.
[0039] The mass ratio of the spherical aluminum powder, the grinding solvent, linoleic acid, isostearic acid, decanol polyoxyethylene ether monoester, the dilution solvent and the coupling agent is 80:160:1.5:1:1:15:0.756.
[0040] In step S1, the spherical aluminum powder has a D50 of 2 μm.
[0041] The grinding solvent used in step S1 includes 150# solvent oil and D70 solvent oil, and the mass ratio of the 150# solvent oil to the D70 solvent oil is 4:1;
[0042] In step S3, the dilution solvent includes D40 solvent oil; and the coupling agent includes isopropyl triisostearyl titanate (CAS (61417-49-0)).
[0043] In step S1 , the grinding medium used is a plurality of bearing steel balls with a diameter of 1.0 mm, and the total mass of all the bearing steel balls is 2000 kg.
[0044] The grinding time in step S1 was 44 h.
[0045] In step S1, the rotation speed of the ball mill is 45 r / min.
[0046] During grinding in step S1, the outer wall temperature of the ball mill does not exceed 50° C. An interlayer is provided on the outer wall of the ball mill, and a water circulation system is provided in the interlayer; if the outer wall temperature of the ball mill exceeds 50° C., the water circulation system is turned on to cool the ball mill, thereby ensuring that the outer wall temperature does not exceed 50° C., and ensuring that the spherical aluminum powder is ground at a suitable temperature.
[0047] The kneading time used in step S3 is 30 minutes.
[0048] The imitation electroplating aluminum paste comprises the following components in percentage by mass:
[0049] The content of aluminum flakes is 65.5%, grinding solvent is 19%, dilution solvent is 14.8%, isostearic acid is 0.2%, decanol polyoxyethylene ether monoester is 0.1% and linoleic acid is 0.4%.
[0050] Based on Example 1, the present invention further prepared Comparative Examples 1-4, wherein Comparative Examples 1-4 were set up with reference to the differences between the prior art and the present invention in preparing aluminum paste products.
[0051] Comparative Example 1:
[0052] The difference from Example 1 is that decanol polyoxyethylene ether monoester is not used.
[0053] Comparative Example 2:
[0054] The difference from Example 1 is that decanol polyoxyethylene ether monoester is not used, and linoleic acid is replaced by oleic acid.
[0055] Comparative Example 3:
[0056] The difference from Example 1 is that decanol polyoxyethylene ether monoester is not used, and isostearic acid is replaced by stearic acid.
[0057] Comparative Example 4:
[0058] The difference from Example 1 is that decanol polyoxyethylene ether monoester is not used, and linoleic acid is replaced by paraffin.
[0059] See also Figure 1In the aluminum paste product prepared in Example 1, the aluminum sheets are closely connected with each other, and the flatness is excellent. Therefore, the paint film has a smooth and silky appearance and excellent water surface coverage.
[0060] See also Figure 2 In the aluminum paste product prepared in Comparative Example 1, there is no connection between the aluminum sheets, resulting in poor paving properties and insufficient compactness. As a result, the appearance of the paint film obviously cannot achieve a silky and delicate effect and excellent water surface coverage.
[0061] See also Figure 3 In the aluminum paste product prepared in Comparative Example 2, the particle size of the aluminum flakes is coarse and the connectivity between the aluminum flakes is poor.
[0062] See also Figure 4 In the aluminum paste product prepared in Comparative Example 3, the particle size of the aluminum flakes is coarse and the connectivity between the aluminum flakes is poor.
[0063] See also Figure 5 In the aluminum paste product prepared in Comparative Example 4, the particle size of the aluminum flakes is coarse and the connectivity between the aluminum flakes is poor.
[0064] The present invention conducted the following tests on the aluminum paste products prepared in Example 1 and Comparative Examples 1-4, and the test results are shown in Table 2. Specifically, in Table 2, the particle size D50 data was compared and tested using Part VII of YS / T617.7-2007: Particle size distribution determination, laser scattering, and diffraction methods (it should be noted that, for the coating industry, the smaller the particle size D50 data, the smoother the paint film appearance);
[0065] The aluminum content data was tested using the second part of YS / T617.2-2007: Determination of aluminum content in aluminum-magnesium alloy powders;
[0066] The water surface coverage rate was tested using the tenth part of YS / T617.10-2007: Determination of the water surface area covered by aluminum powder;
[0067] The L value data of aluminum paste products are determined by the method specified in GB / T9754-2007;
[0068] GB / T21867.1-2008 / ISO8781-1:1990 Pigments and Extenders-Dispersion Evaluation Method is used to test the dispersibility of aluminum paste products;
[0069] GB / 1711-89 pigments were used to compare the thermal stability of aluminum paste products for storage dispersibility, with a storage period of 12 months.
[0070] Table 2 Test results of aluminum paste products obtained in Example 1 and Comparative Examples 1-4
[0071] Experimental protocol Particle size (D50) Aluminum content% <![CDATA[Water surface coverage (cm 2 / g)]]> L value Dispersibility Storage decentralization Example 1 4.23 65.5 48000 103 OK >12 months Comparative Example 1 5.02 65.5 29000 100 OK Less than 12 months Comparative Example 2 5.88 65.5 24000 98 OK 6 months Comparative Example 3 5.21 65.5 20000 98 OK 6 months Comparative Example 4 5.33 65.5 19000 98 OK 6 months
[0072] From the data in Table 2, it can be seen that compared with Comparative Examples 1-4, the present invention can prepare an aluminum paste product with the smallest particle size D50 data, the best water surface coverage, L value and storage dispersibility while ensuring a higher aluminum content by using Example 1. This shows that the combined use of steps S1 to S3 in the present invention can ensure that the prepared product has a whiter color, a fine and silky appearance of the paint film, a strong water surface coverage and good storage dispersibility.
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an electroplating aluminum paste, characterized in that: The following steps are involved: Step S1, adding spherical aluminum powder, grinding solvent, linoleic acid, isostearic acid and decanol polyoxyethylene ether monoester into a ball mill and grinding; Step S2, grinding, screening and filter pressing to prepare aluminum slurry filter cake; Step S3, adding a diluting solvent and a coupling agent to the aluminum paste filter cake, stirring and adding the mixture into a kneader for kneading to obtain a product imitation electroplating aluminum paste; In step S1 and step S3, the mass ratio of the spherical aluminum powder, grinding solvent, linoleic acid, isostearic acid, decanol polyoxyethylene ether monoester, dilution solvent and coupling agent is (75-85): (155-165): (1.5-2): (1-4.0): (1-2): (15-18): (0.7-1.2); The grinding solvent used in step S1 includes 150# solvent oil and D70 solvent oil, and the mass ratio of 150# solvent oil to D70 solvent oil is 4:1~1:1; In step S3, the dilution solvent includes D40 solvent oil; and the coupling agent includes isopropyl triisostearyl titanate.
2. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: In step S1, the spherical aluminum powder is D 50 =1-3μm.
3. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: The grinding medium used in step S1 is a plurality of bearing steel balls with a diameter of 0.6 mm to 1.0 mm.
4. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: The grinding time in step S1 is 35-45 h.
5. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: In step S1, the rotation speed of the ball mill is 45 r / min.
6. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: During the grinding in step S1, the outer wall temperature of the ball mill does not exceed 50°C.
7. The method for preparing the imitation electroplating aluminum paste according to claim 1, characterized in that: The kneading time used in step S3 is 30 minutes.
8. An imitation electroplating aluminum paste prepared by the preparation method of the imitation electroplating aluminum paste as described in any one of claims 1 to 7.