A sodium ion battery and its manufacturing process
The combination of hard carbon/MXene composite materials and layered oxides is used to prepare sodium ion batteries, which solves the problem of poor chemistry of existing sodium ion batteries and achieves higher cycling stability and electrochemical performance improvement.
Patent Information
- Application Number
- CN202211589577.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The chemical performance of existing sodium ion batteries is poor, mainly due to the low conductivity of hard carbon, which causes the electrode to fail during charging and discharging, and lacks effective modification methods to improve electrochemical performance.
Using hard carbon/MXene composite material as the negative electrode active material and layered oxide as the positive electrode active material, sodium ion batteries are prepared through specific preparation processes and assembly methods, avoiding the use of binders and current collectors, thus forming Highly efficient self-supporting electrode.
It effectively improves the cycle stability and electrochemical performance of the battery, significantly improves capacity and energy density, and reduces battery resistance and improves interface performance.
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium ion batteries, and specifically discloses a sodium ion battery and a manufacturing process thereof. Background Art
[0002] Sodium-ion batteries have a similar working principle to lithium-ion batteries, and have become a research hotspot in recent years due to their low raw material costs and abundant reserves. In addition, the negative electrode of sodium-ion batteries can use cheaper aluminum foil, the discharge voltage can reach 0V, and it has good low-temperature performance, and is expected to be used in fields such as smart grids and low-speed vehicles.
[0003] However, graphite, the negative electrode material of lithium-ion batteries, cannot be used in sodium battery systems, so hard carbon has become the first choice for sodium battery negative electrode active materials. However, since the conductivity of hard carbon is lower than that of graphite, the chemical properties of existing sodium-ion batteries are poor. MXene materials, due to their good layered structure, can effectively improve the failure of electrodes caused by volume changes during charging and discharging, and their surface functional groups can improve interface properties. Therefore, there is a need for a sodium-ion battery that can modify the hard carbon negative electrode and has good electrochemical properties. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a sodium ion battery and a manufacturing process thereof.
[0005] The technical solution to achieve the purpose of the present invention is to provide a sodium ion battery and its manufacturing process, using a hard carbon / MXene composite material as a negative electrode active material, using a layered oxide as a positive electrode active material, and making the positive and negative electrode active materials into positive and negative electrode sheets respectively, and assembling them to obtain a sodium ion battery.
[0006] As a further improvement scheme, the hard carbon / MXene negative electrode preparation method is specifically as follows: (1) placing a sucrose solution in a reactor, reacting at 200°C for 6 to 8 hours, cooling and filtering to obtain a precursor material; (2) washing the precursor material with deionized water, dissolving the precursor material in water, mixing it with the MXene solution, and ultrasonically treating it for 2 to 3 hours to obtain a precursor / MXene suspension; (3) freeze-drying the suspension at -40 to -60°C for 2 to 4 hours to obtain a precursor / MXene material; (4) placing the precursor / MXene material in a tubular furnace, high-temperature carbonizing it at 1000 to 1200°C for 4 to 8 hours, and cooling it to obtain a hard carbon / MXene composite material; (5) adding the hard carbon / MXene composite material to an aqueous solution containing a conductive agent, stirring it evenly with a magnetic force, and filtering and vacuum drying the obtained negative electrode slurry in turn to obtain a hard carbon / MXene negative electrode.
[0007] As a further improvement scheme, in the hard carbon / MXene negative electrode, the mass ratio of hard carbon to MXene is (70-90): (10-30).
[0008] As a further improvement scheme, the hard carbon / MXene negative electrode only uses active materials and conductive agents, and does not use current collectors and binders. The mass ratio of hard carbon / MXene active materials to conductive agents is (80-95): (5-20).
[0009] As a further improvement scheme, the positive electrode manufacturing method is specifically as follows: after the layered oxide, the conductive agent and the solvent are uniformly stirred by magnetic force, the prepared positive electrode slurry is filtered and vacuum dried in sequence to obtain the positive electrode.
[0010] As a further improvement, the layered oxide material is Na x TMO 2 , wherein T and M are selected from two or more of nickel (Ni), cobalt (Co), manganese (Mn), iron (Fe), vanadium (V), titanium (Ti), chromium (Cr), copper (Cu), zinc (Zn), and tin (Sn); and the solvent is N-methylpyrrolidone (NMP).
[0011] As a further improvement, the positive electrode uses only active materials and conductive agents, and does not use current collectors or binders. The mass ratio of the layered oxide active material to the conductive agent is (80-95):(5-20).
[0012] As a further improvement, the conductive agent is one or more of conductive carbon black, carbon nanotubes, and graphene.
[0013] As a further improvement plan, the positive electrode sheet and the separator are placed in the battery shell in sequence, the electrolyte is dripped in, the negative electrode is placed on top of the separator, and the gasket, shrapnel and battery shell are placed in sequence to produce a sodium ion battery.
[0014] As a further improvement scheme, the electrolyte consists of a sodium salt and a solvent, the sodium salt is one of sodium hexafluorophosphate and sodium perchlorate, and the solvent is one or more of ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, and fluoroethylene carbonate.
[0015] After adopting the above technical solution, the present invention has the following positive effects:
[0016] (1) In the present invention, MXene material and precursor material are doped at the initial stage of hard carbon production, and then carbonized together to obtain a hard carbon / MXene composite material, which can effectively compound the two materials so that the hard carbon is evenly filled in the MXene structure; compared with simply mechanically mixing hard carbon and MXene, this method can achieve more complete compounding.
[0017] (2) The MXene material of the present invention has a good layered structure, which can effectively improve the failure of the electrode caused by volume change during the charge and discharge process. The functional groups on its surface can improve the interface performance. At the same time, the MXene material has a high specific capacity and can improve the specific capacity of the hard carbon negative electrode.
[0018] (3) The present invention does not use a binder or a current collector in both the positive and negative electrodes. Since the network structure of the conductive agent can produce a good connection effect with the active material, the active material and the conductive agent can be used to form a self-supporting electrode. At the same time, without using a binder or a current collector, the capacity and energy density of the battery can be significantly improved, and the battery resistance can be effectively reduced. DETAILED DESCRIPTION
[0019] Example 1
[0020] 1. Hard carbon / MXene negative electrode production method:
[0021] (1) placing a sucrose solution in a reaction kettle, reacting at 200° C. for 6 h, cooling, and filtering to obtain a precursor material;
[0022] (2) After washing the precursor material with deionized water, the precursor material is dissolved in water and mixed with the MXene solution, and then subjected to ultrasonic treatment for 2 h to obtain a precursor / MXene suspension;
[0023] (3) freeze-drying the suspension at -40 °C for 4 h to obtain a precursor / MXene material;
[0024] (4) placing the precursor / MXene material in a tube furnace, carbonizing it at 1000 °C for 8 h, and then cooling it to obtain a hard carbon / MXene (70:30) composite material;
[0025] (5) The hard carbon / MXene (70:30) composite material is added to an aqueous solution containing a conductive agent, conductive carbon black, and after being evenly stirred by magnetic force, the obtained negative electrode slurry is filtered and vacuum dried in sequence to obtain a hard carbon / MXene (70:30) negative electrode.
[0026] 2. Positive electrode production method:
[0027] 80% layered oxide NaNi 0.72 Fe 0.19 Mn 0.09 O 2 , 20% conductive carbon black, and NMP solvent were stirred evenly by magnetic force, and the prepared positive electrode slurry was filtered and vacuum dried in sequence to obtain the positive electrode.
[0028] 3. Place the positive electrode and separator into the battery shell in turn, and drip (1M NaPF 6 , EC:DEC=1:1) electrolyte, place the negative electrode on the diaphragm, and then put the gasket, shrapnel and battery case in sequence to obtain a sodium ion battery.
[0029] The sodium-ion battery was cycled 100 times at room temperature and 0.5C, with a capacity retention rate of 98.6%.
[0030] 4. Make a half-cell for reversible capacity test, put the hard carbon / MXene (70:30) electrode and diaphragm into the battery shell in turn, and drop (1MNaPF 6 , EC:DEC=1:1) electrolyte, place the sodium sheet on the diaphragm, and then put the gasket, shrapnel and battery shell in sequence to obtain the sodium ion half-cell.
[0031] The capacity of the sodium ion half-battery was tested and the reversible capacity was 339.4 mAh / g.
[0032] Example 2
[0033] 1. Hard carbon / MXene negative electrode production method:
[0034] (1) placing a sucrose solution in a reaction kettle, reacting at 200° C. for 7 h, cooling and filtering to obtain a precursor material;
[0035] (2) After washing the precursor material with deionized water, the precursor material is dissolved in water and mixed with the MXene solution, and then subjected to ultrasonic treatment for 3 h to obtain a precursor / MXene suspension;
[0036] (3) freeze-drying the suspension at -50 °C for 3 h to obtain the precursor / MXene material;
[0037] (4) placing the precursor / MXene material in a tube furnace, carbonizing it at 1100 °C for 6 h, and then cooling it to obtain a hard carbon / MXene (80:20) composite material;
[0038] (5) The hard carbon / MXene (80:20) composite material is added to an aqueous solution containing a conductive agent graphene, and after being evenly stirred by magnetic force, the obtained negative electrode slurry is filtered and vacuum dried in sequence to obtain a hard carbon / MXene (80:20) negative electrode.
[0039] 2. Positive electrode production method:
[0040] 90% layered oxide NaNi 0.29 Fe 0.31 Mn 0.29 Cu 0.11 O 2, 10% conductive agent graphene, and solvent NMP were evenly stirred by magnetic force, and the prepared positive electrode slurry was filtered and vacuum dried in sequence to obtain a positive electrode.
[0041] 3. Place the positive electrode and the separator into the battery shell in turn, and drip (1M NaClO 4 , EC:DEC:EMC=1:1:1) electrolyte, place the negative electrode on the diaphragm, and then put the gasket, shrapnel and battery case in sequence to obtain a sodium ion battery.
[0042] The sodium-ion battery was cycled 100 times at room temperature and 0.5C, with a capacity retention rate of 98.1%.
[0043] 4. Make a half-cell for reversible capacity test. Put the hard carbon / MXene (80:20) electrode and diaphragm into the battery shell in turn, and drip (1M NaClO 4 , EC:DEC:EMC=1:1:1) electrolyte, place the sodium sheet on the diaphragm, and then put the gasket, shrapnel and battery shell in sequence to obtain the sodium ion half-cell.
[0044] The capacity of the sodium ion half-battery was tested and the reversible capacity was 337.1 mAh / g.
[0045] Example 3
[0046] 1. Hard carbon / MXene negative electrode production method:
[0047] (1) placing a sucrose solution in a reaction kettle, reacting at 200° C. for 8 h, cooling, and filtering to obtain a precursor material;
[0048] (2) After washing the precursor material with deionized water, the precursor material is dissolved in water and mixed with the MXene solution, and then subjected to ultrasonic treatment for 3 h to obtain a precursor / MXene suspension;
[0049] (3) freeze-drying the suspension at -60 °C for 2 h to obtain a precursor / MXene material;
[0050] (4) placing the precursor / MXene material in a tube furnace, carbonizing it at 1200 °C for 4 h, and then cooling it to obtain a hard carbon / MXene (90:10) composite material;
[0051] (5) The hard carbon / MXene (90:10) composite material is added to an aqueous solution containing conductive agent graphene + carbon nanotubes (1:2), and after being evenly stirred by magnetic force, the obtained negative electrode slurry is filtered and vacuum dried in sequence to obtain a hard carbon / MXene (90:10) negative electrode.
[0052] 2. Positive electrode production method:
[0053] 95% layered oxide NaNi 0.56 Fe 0.44 O 2 , 5% conductive agent graphene + carbon nanotubes (1:2), and solvent NMP were evenly stirred by magnetic force, and the prepared positive electrode slurry was filtered and vacuum dried in sequence to obtain a positive electrode.
[0054] 3. Place the positive electrode and the separator into the battery shell in turn, and drip (1M NaClO 4 , EC:EMC=1:1) electrolyte, place the negative electrode on the diaphragm, and then put the gasket, shrapnel and battery case in sequence to obtain a sodium ion battery.
[0055] The sodium-ion battery was cycled 100 times at room temperature and 0.5C, with a capacity retention rate of 97.8%.
[0056] 4. Make a half-cell for reversible capacity test. Put the hard carbon / MXene (90:10) electrode and diaphragm into the battery shell in turn, and drip (1M NaClO 4 , EC:EMC=1:1) electrolyte, place the sodium sheet on the diaphragm, and then put the gasket, shrapnel and battery shell in sequence to obtain the sodium ion half-cell.
[0057] The capacity of the sodium ion half-battery was tested and the reversible capacity was 331.6 mAh / g.
[0058] Example 4
[0059] 1. Comparative Example 1
[0060] S1. Negative electrode production method:
[0061] (1) placing a sucrose solution in a reaction kettle, reacting at 200° C. for 6 h, cooling, and filtering to obtain a precursor material;
[0062] (2) After washing the precursor material with deionized water, the precursor material is dissolved in water, and ultrasonically treated for 2 hours to obtain a precursor suspension;
[0063] (3) freeze-drying the suspension at -40°C for 4 h to obtain a precursor material;
[0064] (4) placing the precursor material in a tube furnace, carbonizing it at 1000°C for 8 hours, and then cooling it to obtain a hard carbon material;
[0065] (5) The hard carbon material is added to an aqueous solution containing a conductive agent and conductive carbon black, and after being evenly stirred by magnetic force, the obtained negative electrode slurry is filtered and vacuum dried in sequence to obtain a hard carbon negative electrode.
[0066] S2. Positive electrode production method:
[0067] 80% layered oxide NaNi 0.44 Co 0.31 Mn 0.25 O 2 , 20% conductive carbon black, and NMP solvent were stirred evenly by magnetic force, and the prepared positive electrode slurry was filtered and vacuum dried in sequence to obtain the positive electrode.
[0068] S3. Place the positive electrode and separator into the battery shell in turn, and drip (1M NaPF 6 , EC:DEC=1:1) electrolyte, place the negative electrode on the diaphragm, and then put the gasket, shrapnel and battery case in sequence to obtain a sodium ion battery.
[0069] The sodium-ion battery was cycled 100 times at room temperature and 0.5C, with a capacity retention rate of 85.3%.
[0070] 2. Make a half-battery for reversible capacity test, put the hard carbon electrode and diaphragm into the battery shell in turn, and drip (1M NaPF 6 , EC:DEC=1:1) electrolyte, place the sodium sheet on the diaphragm, and then put the gasket, shrapnel and battery shell in sequence to obtain the sodium ion half-cell.
[0071] The capacity of the sodium ion half-battery was tested and the reversible capacity was 271.4 mAh / g.
[0072] Example 5 Comparison of Examples 1-3 and Comparative Example 1
[0073] (1) The schemes of Examples 1-3 and Comparative Example 1 are as follows:
[0074] plan Hard Carbon: MXene Layered oxides: Conductive agents Freeze drying temperature Carbonization temperature Carbonization time Example 1 70:30 80:20 -40℃ 1000℃ 8h Example 2 80:20 90:10 -50℃ 1100℃ 6h Example 3 90:10 95:5 -60℃ 1200℃ 4h Comparative Example 1 100:0 80:20 -40℃ 1000℃ 8h
[0075] (2) Capacity retention of Examples 1-3 and Comparative Example 1
[0076] Sodium ion battery cycled 100 times at room temperature 0.5C
[0077] plan Example 1 Example 2 Example 3 Comparative Example 1 Capacity retention rate 98.6% 98.1% 97.8% 85.3%
[0078] By comparing the room temperature cycle test data of the sodium ion battery in Examples 1 to 3 with that in Comparative Example 1, it can be seen that the use of a modified hard carbon negative electrode can effectively improve the cycle stability of the battery and enhance the electrochemical performance of the battery.
[0079] (3) Reversible capacity of Examples 1-3 and Comparative Example 1
[0080] plan Example 1 Example 2 Example 3 Comparative Example 1 Reversible capacity mAh / g 339.4 337.1 331.6 271.4
[0081] By comparing the reversible capacity test data of the sodium ion battery in Examples 1 to 3 with that in Comparative Example 1, it can be seen that the use of a modified hard carbon negative electrode can effectively increase the reversible capacity of the battery and improve the electrochemical performance of the battery.
[0082] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for manufacturing a sodium ion battery, Features: A hard carbon / MXene composite material is used as a negative electrode active material, and a layered oxide is used as a positive electrode active material. The positive and negative electrode active materials are respectively made into positive and negative electrode sheets, and a sodium ion battery is obtained after assembly. The specific method for preparing the hard carbon / MXene negative electrode is as follows: (1) placing a sucrose solution in a reactor, reacting it at 200°C for 6 to 8 hours, cooling it, and filtering it to obtain a precursor material; (2) washing the precursor material with deionized water, dissolving the precursor material in water, and mixing it with the MXene solution, and ultrasonically treating it for 2 to 3 hours to obtain a precursor / MXene suspension; (3) freeze-drying the suspension at -40 to -60°C for 2 to 4 hours to obtain a precursor / MXene material; (4) placing the precursor / MXene material in a tubular furnace, high-temperature carbonizing it at 1000 to 1200°C for 4 to 8 hours, and cooling it to obtain a hard carbon / MXene composite material; (5) adding the hard carbon / MXene composite material to an aqueous solution containing a conductive agent, stirring it evenly with a magnetic force, and then filtering and vacuum drying the obtained negative electrode slurry in turn to obtain a hard carbon / MXene negative electrode.
2. The process for producing a sodium ion battery according to claim 1, Features: The hard carbon / MXene negative electrode has a mass ratio of hard carbon to MXene of (70-90): (10-30).
3. The process for producing a sodium ion battery according to claim 1, Features: The hard carbon / MXene negative electrode only uses active materials and conductive agents, and does not use current collectors or binders. The mass ratio of the hard carbon / MXene active materials to the conductive agent is (80-95): (5-20).
4. The process for producing a sodium ion battery according to claim 1, Features: The positive electrode preparation method is specifically as follows: after the layered oxide, the conductive agent and the solvent are uniformly stirred by magnetic force, the prepared positive electrode slurry is filtered and vacuum dried in sequence to prepare the positive electrode.
5. The process for producing a sodium ion battery according to claim 4, Features: The layered oxide material is Na x TMO 2 , wherein T and M are selected from two or more of nickel (Ni), cobalt (Co), manganese (Mn), iron (Fe), vanadium (V), titanium (Ti), chromium (Cr), copper (Cu), zinc (Zn), and tin (Sn); and the solvent is N-methylpyrrolidone (NMP).
6. The process for manufacturing a sodium ion battery according to claim 4, Features: The positive electrode only uses active materials and conductive agents, and does not use current collectors and binders. The mass ratio of the layered oxide active material to the conductive agent is (80-95): (5-20).
7. A process for producing a sodium ion battery according to any one of claims 3 or 6, Features: The conductive agent is one or more of conductive carbon black, carbon nanotubes, and graphene.
8. The process for manufacturing a sodium ion battery according to claim 1, Features: The positive electrode sheet and the separator are placed in the battery shell in sequence, the electrolyte is dripped in, the negative electrode is placed on the separator, and the gasket, the shrapnel and the battery shell are placed in sequence to make a sodium ion battery.
9. The process for manufacturing a sodium ion battery according to claim 8, Features: The electrolyte consists of a sodium salt and a solvent, wherein the sodium salt is one of sodium hexafluorophosphate and sodium perchlorate, and the solvent is one or more of ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, and fluoroethylene carbonate.
10. A sodium ion battery made by the manufacturing process according to any one of claims 1 to 9.