Coating composition and method for producing coating composition
By using a multi-layer structure of scaly evaporated metallic pigments in the coating composition, a coating film with high brightness and light color tone is formed, which solves the difficulty in meeting the needs for unique design and high-end feel in the automotive coating field in the existing technology. Achieving higher brightness and uniquely designed coating effects.
Patent Information
- Application Number
- CN202180046449.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-21
AI Technical Summary
It is difficult to form a coating film with a unique design that has the brightness and light color of previous metal coating films with existing technology. Especially in the field of automotive coatings, it is difficult to meet consumers' demands for a high-end feel and unique design.
A coating composition containing scaly evaporated metallic pigments is used. The scaly evaporated metallic pigments have a first protective layer, a evaporated metal layer and a second protective layer, with an average particle size of 10 to 150 μm and an average thickness of 0.5 to 10 μm. Aspect ratio is 5 ~50, the first protective layer and the second protective layer contain silicone components, the light intensity of the cured coating film of the coating composition at an incident angle of 45° is more than 5, the bright area is more than 10, and the granularity value is more than 5 and less than 10 , the chroma C* is less than 5.
It forms a brighter coating film with a unique design and light color tone to meet consumers' needs for high-end and uniqueness.
Abstract
Description
Technical Field
[0001] The present invention relates to a coating composition and a method for producing the coating composition. Background Art
[0002] A variety of coatings with various functions are sequentially formed on the surface of the coated object such as the automobile body, which gives a beautiful appearance and excellent design while protecting the coated object. As a method for forming such a variety of coatings, a primer coating such as an electrodeposition coating is generally formed on the coated object with excellent conductivity, and a middle coating film and an upper coating film are sequentially formed thereon as required. Among these coatings, the upper coating film composed of a base coating film and a clear coating film has a particularly large impact on the appearance and design of the coating film. In particular, in automobiles, the appearance and design of the upper coating film composed of a base coating film and a clear coating film formed on the vehicle body are extremely important.
[0003] The base coating can be roughly divided into a coating without flaky pigments, which is called a so-called pure color, and a coating containing flaky pigments with a glossy feel. A representative example of a flaky pigment with a glossy feel is a flaky aluminum pigment. By including a flaky aluminum pigment in the base coating, a metallic luster (metallic feel) can be expressed.
[0004] In recent years, in the field of automobile painting, the development of coatings with high design has been carried out. This is because consumers tend to prefer coatings with a visible glossy feeling that gives a sense of luxury, rather than so-called solid colors. Furthermore, in response to the diversification of consumer preferences and the desire for uniqueness, consumers are demanding not only simple glossiness, but also more unique designs such as coatings with higher brightness than the previous glossiness.
[0005] WO2019 / 131957 specification (Patent Document 1) describes a coating composition comprising a binder component (A), a flaky aluminum pigment (B) having an average particle size (d50) in the range of 18 to 25 μm, and a flaky pigment (C) other than the flaky aluminum pigment having an average particle size (d50) in the range of 8 to 30 μm. It is described that by using the coating composition, a coating film having a high granular feel and suppressing the generation of metal unevenness can be formed.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: WO2019 / 131957 Specification Summary of the invention
[0009] Problems to be solved by the invention
[0010] Patent Document 1 describes that a coating film having a high graininess and suppressed metallic unevenness can be formed by using a specific flaky aluminum pigment (B) and a flaky pigment (C) other than the flaky aluminum pigment in combination and using the coating composition described.
[0011] On the other hand, an object of the present invention is to provide a coating film having a unique design and exhibiting a light color tone while having the brilliance exhibited by conventional metal coating films.
[0012] Methods for solving problems
[0013] In order to solve the above-mentioned problems, the present invention provides the following aspects.
[0014] [1] A coating composition comprising a coating film-forming resin and a pigment, wherein the pigment comprises a flaky vapor-deposited metal pigment, and a cured coating film of the coating composition has a luminous intensity (Si) of 5 or more at an incident angle of 45°, a luminous area (Sa value) of 10 or more, a granularity value (G value) of 5 or more and 10 or less, and a chroma C* of 5 or less at an incident angle of 45° and a light receiving angle of 45°.
[0015] [2] The coating composition according to [1], wherein the angle-dependent angular flop value of the cured coating film is 1.1 or more and less than 2.
[0016] [3] The coating composition according to [1] or [2], wherein the flaky vapor-deposited metal pigment comprises a first protective layer, a vapor-deposited metal layer and a second protective layer in sequence, and the flaky vapor-deposited metal pigment has an average particle size of 10 to 150 μm, an average thickness of 0.5 to 10 μm, and an aspect ratio of 5 to 50.
[0017] [4] The coating composition according to [3], wherein the average thickness of each of the first protective layer and the second protective layer is 0.5 to 3 μm, and the average thickness of the vapor-deposited metal layer is 5 to 100 nm.
[0018] [5] The coating composition according to [3] or [4], wherein the first protective layer and the second protective layer each contain a silicone component.
[0019] [6] The coating composition according to any one of [3] to [5], wherein the deposited metal layer contains aluminum.
[0020] [7] The coating composition according to any one of [1] to [6], wherein the amount of the flaky deposited metal pigment contained in the coating composition is in the range of 0.1 to 40 parts by mass relative to 100 parts by mass of the resin solid content of the coating film forming resin.
[0021] [8] A method for producing a cured coating film, comprising the steps of applying the coating composition described in any one of [1] to [7] to a coated object and then heating and curing the object, wherein the cured coating film has a luminous intensity (Si) of 5 or more at an incident angle of 45°, a luminous area (Sa value) of 10 or more, a granularity value (G value) of 5 or more and 10 or less, and a chroma C* of 5 or less at an incident angle of 45° and a light receiving angle of 45°.
[0022] [9] An article comprising a cured coating film of the coating composition according to any one of [1] to [7].
[0023] Effects of the Invention
[0024] By using the above coating composition, a coating film having higher brightness can be formed compared with a coating film formed from a conventional metallic coating composition. DETAILED DESCRIPTION
[0025] The coating composition comprises a coating film forming resin and a pigment. Here, it is characterized in that the pigment comprises a flaky vapor-deposited metal pigment, and the luminous intensity (Si) of the cured coating film of the coating composition at an incident angle of 45° is 5 or more, the luminous area (Sa value) is 10 or more, the granularity value (G value) is 5 or more and 10 or less, and the chroma C* is 5 or less. The components contained in the coating composition are described below.
[0026] pigment
[0027] It is characterized in that the coating composition contains a pigment, and the pigment contains a flaky vapor-deposited metal pigment. The pigment may contain other pigments other than the flaky vapor-deposited metal pigment as required. As other pigments, for example, coloring pigments and extender pigments can be listed. As coloring pigments, inorganic coloring pigments such as titanium dioxide, carbon black, iron oxide, yellow iron oxide, and various organic coloring pigments can be listed, such as phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green, azo pigments such as azo red, azo yellow, and azo orange, quinacridone pigments such as quinacridone red, Cinquasia Red, and Cinquasia magenta, perylene pigments such as perylene red and perylene maroon, carbazole violet, anthrapyridine, flavanone yellow, isoindoline yellow, indanthrone blue, dibromoanthraquinone red, anthraquinone red, diketopyrrolopyrrole, etc. As extender pigments, for example, calcium carbonate, barium sulfate, clay, talc, etc. can be cited. The above-mentioned pigment may further contain an anti-rust pigment as required.
[0028] In addition, as required, the pigment may contain flaky metal pigments other than flaky vapor-deposited metal pigments. Examples of such pigments include metallic bright pigments (crushed metallic bright pigments) such as aluminum, copper, zinc, iron, nickel, tin, aluminum oxide, and alloys thereof, interference mica pigments, muscovite pigments, graphite pigments, and glass flake pigments.
[0029] When the above pigment is contained, it is provided that the effect of the present invention is not impaired. The above pigment can be contained in an amount of, for example, 0.1 to 30 parts by mass relative to 100 parts by mass of the resin solid content.
[0030] Flake-like vapor-deposited metallic pigments
[0031] The flaky vapor-deposited metal pigment is a flaky pigment having a vapor-deposited metal layer. The flaky vapor-deposited metal pigment is preferably a pigment having a first protective layer, a vapor-deposited metal layer, and a second protective layer in this order.
[0032] The above-mentioned flaky vapor-deposited metal pigment can be produced, for example, by forming a release layer on a resin substrate, then vapor-depositing a metal layer, and then peeling and pulverizing the metal layer in a solvent to obtain a flaky powder dispersion containing flaky powder. In addition, in the above-mentioned production steps, by containing a protective layer forming component in the flaky powder dispersion, a flaky vapor-deposited metal pigment having a first protective layer, a vapor-deposited metal layer, and a second protective layer in sequence can be appropriately prepared.
[0033] Examples of the resin substrate that can be used for producing the flaky vapor-deposited metal pigment include polyethylene terephthalate (PET) films, polyethylene naphthalate (PEN) films, and polycarbonate (PC) films.
[0034] As the above-mentioned release layer forming component, a resin that is soluble in the solvent contained in the flaky powder dispersion, such as cellulose acetate butyrate resin and polyvinyl acetal resin, can be preferably used. The release layer forming component can be applied on the resin substrate by a wet coating method (such as a gravure coating method) that can be generally used by those skilled in the art to form a release layer. The concentration of the resin contained in the release layer forming component can be appropriately selected according to the type of resin. The thickness of the release layer is preferably in the range of 30 to 100 nm in terms of dry film thickness.
[0035] Examples of the metal deposited on the release layer include aluminum, copper, gold, silver, copper, zinc, titanium, chromium, nickel, nickel-chromium, stainless steel, and mixtures and alloys thereof (e.g., brass, etc.). As the metal, aluminum can be preferably used from the viewpoints of availability and ease of handling.
[0036] The metal layer can be formed by a dry coating method (e.g., sputtering, vacuum evaporation, etc.) that can be generally used by those skilled in the art. The evaporation conditions can be appropriately selected according to the type of metal, etc. The thickness of the metal layer is preferably in the range of 5 to 100 nm, more preferably in the range of 20 to 75 nm.
[0037] The solvent that can be used to strip the metal layer in the solvent is a solvent that can at least partially dissolve the release layer. As the solvent, for example, ester solvents such as butyl acetate, ketone solvents such as acetone, etc. can be preferably used. The stripping of the metal layer can be performed by immersing the resin substrate formed with the release layer and the metal layer in the solvent, and scraping the metal layer laminated on the surface of the resin substrate using, for example, a scraper.
[0038] As a method for pulverizing the above-mentioned metal layer in a solvent, a wet pulverization method that can be generally used by a person skilled in the art can be cited. For example, it can be pulverization using an ultrasonic homogenizer, and it can also be a method of coarse pulverization using a homogenizer and fine pulverization using a high-pressure homogenizer. The pulverization here is preferably carried out in a manner that the average particle size (average major diameter) of the obtained flaky vapor-deposited metal pigment is within the range of 10 to 150 μm.
[0039] In this specification, the average particle size (average major diameter) of the flaky vapor-deposited metallic pigment can be measured by observing the flaky vapor-deposited metallic pigment using a shape analysis laser microscope (e.g., VK-X250 manufactured by KEYENCE) and determining the number average of the maximum length (major diameter) of 100 randomly selected pigments.
[0040] The state after the pulverization is the state of a dispersion in which the pulverized deposited metal layer is dispersed in a scale-like state. By including a protective layer forming component in the dispersion, a protective layer can be provided on the scale-like deposited metal layer. Thus, a scale-like deposited metal pigment having a first protective layer, a deposited metal layer, and a second protective layer in sequence can be appropriately prepared.
[0041] As the above-mentioned protective layer forming component, for example, silane coupling agents, siloxane compounds, etc. can be preferably used. As a silane coupling agent, for example, a silane coupling agent having one or more organic functional groups selected from the group consisting of epoxy, amino and isocyanate groups is preferably used, and a silane coupling agent having an epoxy group is more preferably used. As a siloxane compound, carboxyl-containing siloxane compounds can be listed. They can be used only one, or two or more can be used in combination. It should be noted that when the protective layer is formed by the above steps, the protective layer may contain a resin component (such as cellulose acetate butyrate resin, polyvinyl alcohol acetal resin, etc.) of a release agent. Through the above steps, it is possible to appropriately prepare a flaky evaporated metal pigment having a first protective layer, an evaporated metal layer and a second protective layer in sequence, and the first protective layer and the second protective layer respectively contain a pigment of an organic silicon component.
[0042] In the formation of the above-mentioned protective layer, coloring can be performed as needed. For example, by using a silane coupling agent as a protective layer forming component, and then containing an organic coloring pigment in the dispersion, a colored protective layer can be formed. As an organic coloring pigment, the above-mentioned organic coloring pigment can be used. As an organic coloring pigment, more specifically, polycyclic pigments such as condensed ring compounds (such as phthalocyanine pigments, etc.), azo pigments having double bonds between nitrogen atoms, etc. can be cited. By using such an organic coloring pigment, a flaky vapor-deposited metal pigment can be obtained in which the first protective layer and the second protective layer respectively contain an organosilicon component and the above-mentioned protective layer is colored.
[0043] The flaky vapor-deposited metal pigment preferably has a first protective layer, a vapor-deposited metal layer, and a second protective layer in sequence, wherein the average thickness of each layer of the first protective layer and the second protective layer is preferably 0.5 to 3 μm. The average thickness of each layer of the first protective layer and the second protective layer can be adjusted by adjusting the concentration of the protective layer-forming component to a suitable range. For example, a method of adjusting the concentration of the protective layer-forming component contained in the dispersion to a range of 0.1 to 5 parts by mass relative to 100 parts by mass of the metal layer contained in the dispersion can be cited.
[0044] The average thickness of the flaky vapor-deposited metallic pigment is preferably 0.5 to 10 μm. The average thickness of the flaky vapor-deposited metallic pigment can be measured by forming a coating film including the flaky vapor-deposited metallic pigment, measuring a cross section of the obtained coating film using a transmission electron microscope (TEM), and finding the average of the measured values.
[0045] The aspect ratio of the scaly vapor-deposited metallic pigment is preferably in the range of 5-50.
[0046] As the above-mentioned flaky vapor-deposited metal pigment, a commercial product can be used. As a commercial product, for example, the Elgee neo series (e.g., #200, #325, #500, etc.) manufactured by Oike Industries can be listed, and as a particularly preferred product, the Elgee neo Extra White series can be listed. As a commercial product, other commercial products manufactured by the same method as the above method can be used.
[0047] The amount of the flaky vapor-deposited metal pigment contained in the coating composition is preferably in the range of 0.1 to 40 parts by mass, more preferably 1 to 40 parts by mass, and even more preferably 3 to 40 parts by mass, based on 100 parts by mass of the resin solid content.
[0048] Film forming resin
[0049] The coating composition contains a coating film forming resin. Examples of the coating film forming resin include acrylic resins, polyester resins, polyurethane resins, epoxy resins, fluororesins, silicone resins, etc. The coating composition may be a water-based coating composition or a solvent-based coating composition.
[0050] When the above-mentioned coating composition is an aqueous coating composition, as a coating film forming resin, for example, preferably comprises an acrylic resin emulsion (also comprising an acrylic silicone resin emulsion, an acrylic polyurethane resin emulsion, etc.), an acrylic resin dispersion (also comprising an acrylic silicone resin dispersion, an acrylic polyurethane resin dispersion, etc.), a water-soluble acrylic resin, a polyester resin dispersion, a polyurethane resin dispersion, an epoxy resin dispersion, etc. These resins can only be used alone, or two or more thereof can be used in combination. The above-mentioned resin can be prepared by the method commonly used by those skilled in the art. As the above-mentioned resin, a commercially available product can be used.
[0051] Preferred embodiments include, for example, an embodiment using either or both of an acrylic resin emulsion and a water-soluble acrylic resin, an embodiment using an acrylic resin emulsion, a water-soluble acrylic resin, and a polyester resin dispersion, and an embodiment using an acrylic resin emulsion, a water-soluble acrylic resin, and a polyurethane resin dispersion.
[0052] The acrylic resin emulsion can be prepared, for example, by emulsion polymerization of an α,β-ethylenically unsaturated monomer mixture. Preferred α,β-ethylenically unsaturated monomers used in the preparation of the acrylic resin emulsion include, for example, (meth)acrylates, α,β-ethylenically unsaturated monomers having an acid group, and α,β-ethylenically unsaturated monomers having a hydroxyl group.
[0053] Examples of the (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dihydrodicyclopentadienyl (meth)acrylate. It should be noted that in the present specification, the (meth)acrylate refers to both acrylate and methacrylate.
[0054] Examples of the α,β-ethylenically unsaturated monomer having an acid group include acrylic acid, methacrylic acid, crotonic acid, 2-acryloyloxyethylphthalic acid, 2-acryloyloxyethylsuccinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, 2-acrylamide-2-methylpropanesulfonic acid, p-hydroxystyrene, and 2,4-dihydroxy-4′-vinylbenzophenone.
[0055] Examples of the α,β-ethylenically unsaturated monomer having a hydroxyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methallyl alcohol, and adducts thereof with ε-caprolactone, etc. Among them, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyethyl (meth)acrylate, and adducts thereof with ε-caprolactone are preferred.
[0056] The above-mentioned α,β-ethylenically unsaturated monomer mixture can further use other α,β-ethylenically unsaturated monomers. As other α,β-ethylenically unsaturated monomers, polymerizable amide compounds, polymerizable aromatic compounds, polymerizable nitriles, polymerizable oxyalkylene compounds, multifunctional vinyl compounds, polymerizable amine compounds, α-olefins, dienes, polymerizable carbonyl compounds, polymerizable alkoxysilyl compounds, and other polymerizable compounds can be cited. The above-mentioned α,β-ethylenically unsaturated monomers can be variously selected according to the purpose as needed.
[0057] The acrylic resin emulsion can be prepared by emulsion polymerization of the above-mentioned α, β-ethylenically unsaturated monomer mixture. Emulsion polymerization is not particularly limited and can be carried out using a common method. Specifically, for example, it can be carried out as follows: an emulsifier is dissolved in an aqueous medium containing water or an organic solvent such as an alcohol, ether (such as dipropylene glycol methyl ether, propylene glycol methyl ether, etc.) as required, and the above-mentioned α, β-ethylenically unsaturated monomer mixture and a polymerization initiator are added dropwise under heating and stirring. An α, β-ethylenically unsaturated monomer mixture pre-emulsified with an emulsifier and water can also be added dropwise in the same manner.
[0058] The above-mentioned polymerization initiator and emulsifier can use substances commonly used by those skilled in the art. If necessary, chain transfer agents such as mercaptans such as lauryl mercaptan and α-methylstyrene dimer can be used to adjust the molecular weight. The reaction temperature, reaction time, etc. can be appropriately selected within the range commonly used by those skilled in the art. The acrylic resin emulsion obtained by the reaction can be neutralized with a base as needed.
[0059] The lower limit of the number average molecular weight of the acrylic resin emulsion is preferably 3000. In addition, the hydroxyl value (solid content hydroxyl value) of the acrylic resin emulsion preferably has a lower limit of 20 mgKOH / g and an upper limit of 180 mgKOH / g, and the acid value (solid content acid value) preferably has a lower limit of 1 mgKOH / g and an upper limit of 80 mgKOH / g.
[0060] In this specification, the number average molecular weight is a value determined by the GPC method using polystyrene as a standard. In this specification, the acid value and the hydroxyl value are values calculated from the monomer composition used in the preparation based on the provisions of JIS.
[0061] The water-soluble acrylic resin can be prepared, for example, by solution polymerization of a monomer mixture containing α,β-ethylenically unsaturated monomers that can be used in the preparation of the acrylic resin emulsion, and then dissolving it in water using a basic compound. The acrylic resin dispersion can be prepared, for example, by solution polymerization of a monomer mixture containing α,β-ethylenically unsaturated monomers that can be used in the preparation of the acrylic resin emulsion, and then dispersing it using a basic compound.
[0062] A polyester resin dispersion can be prepared, for example, by condensing a polyol component with a polyacid component and dispersing it with a basic compound. A polyurethane resin dispersion can be prepared, for example, by polymerizing a polyol compound, a compound having an active hydrogen group and a hydrophilic group in the molecule, and an organic polyisocyanate using a chain extender and a polymerization terminator as required, and dissolving or dispersing the obtained polymer in water.
[0063] In the case where the above-mentioned coating composition is an aqueous coating composition, it is preferred to use a curing agent that forms a resin reaction with the above-mentioned film. As a curing agent, melamine resin, blocked isocyanate compound, epoxy compound, aziridine compound, carbodiimide compound, oxazoline compound, metal ion, etc. can be used. They can only be used alone 1 kind, and 2 kinds or more thereof can also be used in combination. The above-mentioned components can be prepared by the method commonly used by those skilled in the art. As the above-mentioned components, a commercially available product can be used. As a curing agent, it is more preferred to use any one or both of melamine resin and blocked isocyanate compound.
[0064] Melamine resin can use water-soluble melamine resin and / or water-insoluble melamine resin.Melamine resin is contained in the structure that hydrogen atom or substituent (alkyl ether group, methylol etc.) is bonded to around melamine core (triazine core) via 3 nitrogen atoms.Above-mentioned melamine resin is usually made of the multinuclear body that a plurality of melamine cores are bonded to each other.On the other hand, above-mentioned melamine resin can also be the mononuclear body that is made of 1 melamine core.
[0065] As the above-mentioned melamine resin, commercially available products can be used. As specific examples of commercially available products, for example, CYMEL series (trade names) manufactured by Allnex can be listed, and specifically, CYMEL202, CYMEL204, CYMEL211, CYMEL232, CYMEL235, CYMEL236, CYMEL238, CYMEL250, CYMEL251, CYMEL254, CYMEL266, CYMEL267, CYMEL272, CYMEL285, CYMEL301, CYMEL303, CYMEL325, CYMEL327, CYMEL350, CYMEL370, CYMEL701, CYMEL703, CYMEL1141 and U-VAN (trade name) series manufactured by Mitsui Chemicals can be listed. These can be used alone or in combination of two or more.
[0066] The blocked isocyanate compound can be prepared by adding a blocking agent having active hydrogen to a polyisocyanate including trimethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, etc. Such a blocked isocyanate resin is heated to dissociate the blocking agent to generate an isocyanate group, which reacts with the functional group in the above resin component to cure.
[0067] The amount of the curing agent is preferably 5 to 100 parts by mass, more preferably 10 to 80 parts by mass, based on 100 parts by mass of the solid content of the coating film forming resin.
[0068] In addition to the above-mentioned components, the aqueous coating composition may also include additives commonly used by those skilled in the art, such as surface conditioners, viscosity control agents, thickeners, antioxidants, UV protection agents, defoamers, etc. For example, by using a viscosity control agent, thixotropy can be imparted and coating workability can be adjusted. As a viscosity control agent, for example, crosslinked or non-crosslinked resin particles, swelling dispersions of fatty acid amides, amide-based fatty acids, polyamide-based materials such as phosphates of long-chain polyaminoamides, materials such as polyethylene systems such as colloidal swelling dispersions of oxidized polyethylene, organic acid montmorillonite clays, montmorillonite, etc. can be cited. When using these additives, it can be used in the amount commonly used by those skilled in the art.
[0069] In addition to the above-mentioned components, the above-mentioned water-based coating composition may further contain an organic compound containing a phosphoric acid group. By containing an organic compound containing a phosphoric acid group, there are advantages such as improved dispersibility of the pigment. Furthermore, for example, when the coating film is formed, there are advantages such as being able to well control the orientation of the above-mentioned flaky vapor-deposited metal pigment.
[0070] The aqueous coating composition may contain water and, if necessary, a water-soluble or water-miscible organic solvent as a solvent.
[0071] The above-mentioned water-based coating composition can be produced by a method commonly used by those skilled in the art such as mixing and dispersing the above-mentioned flaky vapor-deposited metal pigment, the coating film-forming resin, the curing agent, and other pigments as needed, the organic compound containing a phosphoric acid group, and additives using a disperser, a homogenizer, a kneader, etc. In the above-mentioned production method, for example, it is preferred to prepare the flaky vapor-deposited metal pigment and the organic compound containing a phosphoric acid group as needed in advance and mix them.
[0072] When the coating composition is a solvent-based coating composition, examples of the coating film-forming resin include acrylic resins, polyester resins (including urethane-modified polyester resins, etc.), etc. These resins may be used alone or in combination of two or more.
[0073] The acrylic resin can be prepared, for example, by solution polymerization of a monomer mixture containing α,β-ethylenically unsaturated monomers. The number average molecular weight of the acrylic resin is preferably 1000 to 20000. In addition, the acid value (solid content acid value) of the acrylic resin is preferably 1 to 80 mgKOH / g, more preferably 10 to 45 mgKOH / g. In addition, the hydroxyl value (solid content hydroxyl value) is preferably 10 to 200 mgKOH / g.
[0074] As the acrylic resin, a commercially available product may be used, and examples of the commercially available product include DIANAL HR series manufactured by Mitsubishi Rayon Co., Ltd.
[0075] The amount of the acrylic resin is preferably 30 to 80% by mass, more preferably 35 to 70% by mass, based on the solid content mass of the coating resin (solid content mass of the coating film forming component).
[0076] As the polyester resin, for example, a hydroxyl-containing polyester resin can be used. The hydroxyl-containing polyester resin can be prepared by polycondensing an acid component such as a polycarboxylic acid and / or an acid anhydride with a polyol.
[0077] When the above-mentioned coating composition is a solvent-based coating composition, it is preferred to use a curing agent that reacts with the above-mentioned coating film to form a resin. As a curing agent, melamine resin, blocked isocyanate compounds, etc. can be used. They can be used alone or in combination of two or more. The above-mentioned components can be prepared by the method commonly used by those skilled in the art. As the above-mentioned components, commercially available products can be used.
[0078] The curing agent preferably contains melamine resin. As melamine resin, there is no particular limitation, and methylated melamine resin, butylated melamine resin, methyl / butyl mixed melamine resin, etc. can be used. For example, the Cymel series commercially available from Allnex and the U-VAN series commercially available from Mitsui Chemicals can be cited. The amount of melamine resin is based on the solid content mass of the coating resin (the solid content mass of the coating film forming component), preferably 10 to 50% by mass, more preferably 15 to 40% by mass.
[0079] The curing agent preferably further comprises a blocked isocyanate compound. The blocked isocyanate compound can be prepared by reacting a blocked compound such as a compound having an active methylene group, a ketone compound or a caprolactam compound with a polyisocyanate. As the blocked isocyanate compound, a commercially available product can be used. As a commercially available product, for example, the Duranate series manufactured by Asahi Chemical Industry Co., Ltd., the Sumidur series manufactured by Sumika Covestro Urethane Co., Ltd., etc. can be cited.
[0080] The amount of the blocked isocyanate compound contained in the coating composition is preferably 10 to 30% by mass, more preferably 15 to 25% by mass, based on the coating resin solid content mass (solid content mass of coating film forming components).
[0081] The solvent-based coating composition may contain, in addition to the above-mentioned components, additives commonly used by those skilled in the art, such as curing catalysts, surface conditioners, ultraviolet absorbers, antioxidants, and the like.
[0082] The solvent-based coating composition can be appropriately adjusted in solid content concentration and viscosity by diluting it with an organic solvent during coating. Examples of usable organic solvents include ester solvents, ether solvents, alcohol solvents, ketone solvents, aliphatic hydrocarbon solvents, aromatic solvents, and the like.
[0083] The solvent-based coating composition may further contain an organic compound containing a phosphoric acid group in addition to the above-mentioned components. The organic compound containing a phosphoric acid group has advantages such as improved dispersibility of the pigment. Furthermore, for example, when the coating film is formed, it has advantages such as being able to well control the orientation of the flaky vapor-deposited metal pigment.
[0084] The above-mentioned solvent-based coating composition can be produced by a method commonly used by those skilled in the art, such as kneading and dispersing the above-mentioned flaky vapor-deposited metal pigment, the coating film-forming resin, the curing agent, and other pigments, organic compounds containing phosphoric acid groups, and additives as required, using a disperser, a homogenizer, a kneader, etc. In the above-mentioned production method, for example, it is preferred to prepare in advance a paste containing the flaky vapor-deposited metal pigment and, as required, the organic compound containing phosphoric acid groups and / or the pigment dispersant and mix them.
[0085] Film formation
[0086] The object to be coated as the object of the coating composition is not particularly limited, and for example, metals, plastics, foams, etc. can be cited. The coating composition can be particularly advantageously used for metals and castings, and can be particularly suitable for metals that can be electrodeposited. As such metals, for example, iron, copper, aluminum, tin, zinc, etc. and alloys containing these metals can be cited. These coated objects can also be molded objects. As specific examples of molded objects, for example, automobile bodies and parts thereof such as passenger cars, trucks, motorcycles, and buses can be cited. The above-mentioned metal and other coated objects are more preferably pre-treated with a phosphoric acid-based chemical treatment agent, a zirconium-based chemical treatment agent, etc. before electrodeposition coating. It is preferred that a cured electrodeposition coating film is formed on the coated object that has been subjected to a chemical treatment as required. As an electrodeposition coating composition for forming a cured electrodeposition coating film, any of a cationic type and an anionic type can be used. By using a cationic electrodeposition coating composition as an electrodeposition coating composition, a coating film with better corrosion resistance can be formed, so it is preferred.
[0087] The above-mentioned coated object can further form a mid-coat film on the cured electrodeposition coating film as needed. A mid-coat coating composition is used in the formation of the mid-coat coating film. As the mid-coat coating composition, for example, a coating composition containing a film-forming resin, a curing agent, various coloring components of an organic system and / or an inorganic system, and a body pigment can be used. The film-forming resin and the curing agent are not particularly limited. Specifically, the film-forming resin and the curing agent listed in the above-mentioned water-based coating composition can be used. As the film-forming resin of the mid-coat coating composition, from the viewpoint of various properties of the obtained mid-coat coating film, it is preferred to use a combination of an acrylic resin and / or a polyester resin and an amino resin and / or an isocyanate.
[0088] Examples of the coloring components contained in the mid-coat include coloring components mainly composed of carbon black and titanium dioxide (gray mid-coat compositions), coloring components mainly composed of titanium dioxide (white mid-coat compositions), and coloring components having a hue similar to that of the top base coating (so-called colored mid-coat compositions).
[0089] The coating composition can be applied to the object by a method commonly used in the field of coatings. As the coating method, for example, pneumatic atomization coating, airless atomization coating, electrostatic atomization coating, multi-stage coating (preferably 2-stage coating) based on pneumatic electrostatic atomization coating, coating combining pneumatic electrostatic atomization coating with a rotary atomization electrostatic coating machine, etc. can be cited.
[0090] The coating composition is preferably applied so as to have a dry film thickness within a range of 3 to 20 μm.
[0091] As a coating film formation method using the said coating composition, the following method is mentioned, for example.
[0092] A method of applying the above coating composition and curing it by heating. After curing by heating, a clear coating film can be formed as required.
[0093] A method in which the above-mentioned coating composition is applied to form an uncured coating film, a clear coating composition is then applied to form an uncured clear coating film, and the obtained uncured coating film is cured by heating at one time.
[0094] A method of forming a coating film by applying the above-mentioned coating composition and then drying it at room temperature. If necessary, for example, a reaction-curable clear coating composition may be applied to form a clear coating film.
[0095] The heating temperature and time when the coating composition is applied and heated to cure can be appropriately selected according to the composition (water-based or solvent-based) of the coating composition and the type of the object to be coated. The heating temperature can be appropriately selected in the range of, for example, 80 to 180° C., preferably 100 to 160° C., etc. The heating time can be appropriately selected in the range of, for example, 5 minutes to 60 minutes, preferably 10 minutes to 30 minutes, etc.
[0096] The clear coating composition is not particularly limited, and examples thereof include solvent-based, water-based, and powder-based clear coating compositions.
[0097] Preferred examples of the solvent-based clear coating composition include, from the perspectives of transparency and acid etching resistance, combinations of acrylic resins and / or polyester resins with amino resins and / or isocyanates, or acrylic resins and / or polyester resins having a carboxylic acid / epoxy curing system.
[0098] Examples of water-based clear coating compositions include those containing a resin made water-based by neutralizing the film-forming resin cited as an example of the above-mentioned solvent-based clear coating composition with a base. The neutralization can be performed by adding a tertiary amine such as dimethylethanolamine and triethylamine before or after polymerization.
[0099] In order to ensure coating workability, these solvent-based clear coating compositions and water-based clear coating compositions preferably contain a viscosity control agent. The viscosity control agent can generally use a substance showing thixotropy. As examples of the viscosity control agent, for example, the viscosity control agents listed in the water-based coating composition can be used. In addition, additives commonly used in the coating field can also be contained as needed.
[0100] As the powder type clear coating composition, for example, a powder coating composition commonly used in the coating field such as a thermoplastic powder coating composition and a thermosetting powder coating composition can be used. Among them, a thermosetting powder coating composition is preferred from the perspective of coating film properties. Specific examples of the thermosetting powder coating composition include epoxy-based, acrylic-based, and polyester-based clear coating compositions.
[0101] The clear coating composition can be applied by a coating method known to those skilled in the art according to the coating form of the clear coating composition. The dry film thickness of the clear coating film formed by applying the clear coating composition is usually preferably 10 to 80 μm, more preferably 20 to 60 μm.
[0102] The uncured clear coating film obtained by the application of the clear coating composition is heat-cured to form a cured clear coating film. When the clear coating composition is applied to the uncured second base coating film, these uncured coating films are heat-cured by heating. From the viewpoint of curability and the physical properties of the obtained multilayer coating film, the heat-curing temperature is preferably set to 80 to 180° C., and is further preferably set to 120 to 160° C. The heat-curing time can be arbitrarily set according to the above temperature. As heat-curing conditions, for example, conditions of heating for 10 minutes to 30 minutes at a heat-curing temperature of 120° C. to 160° C. can be cited.
[0103] Depending on the type of coating composition, after applying the coating composition, it may be dried at room temperature to form a coating film, and then, for example, a reaction-curable clear coating composition may be applied to form a clear coating film.
[0104] The present invention is based on the conditions that the luster intensity (Si) of the cured coating film formed by applying the above-mentioned coating composition at an incident angle of 45° is greater than 5, the luster area (Sa value) is greater than 10, the granularity value (G value) is greater than 5 and less than 10, and the chroma C* is less than 5.
[0105] The above-mentioned gloss intensity (Si) is an index indicating the gloss intensity, and the higher the value, the stronger the gloss. The gloss area (Sa value) is an index that numerically represents the area (size) of the glossy portion. The granularity value (G value) is an index that numerically represents the granularity in the coating film.
[0106] In this specification, the measurements of the above-mentioned gloss intensity (Si), gloss area (Sa value) and granularity value (G value) refer to the values measured using a coating film having a film thickness of 15 μm as a cured coating film of the above-mentioned coating composition. More specifically, on a steel plate coated with a cationic electrodeposition coating composition, on a coated plate having a cured intermediate coating film having a brightness of 60, the above-mentioned coating composition is sprayed in a manner of a coating film of 15 μm, and then a clear coating composition is sprayed in a manner of a film thickness of 35 μm, and then heat-cured at 140° C. for 20 minutes, and the measurement is performed using the cured coating film obtained in this manner.
[0107] The brightness of the cured intermediate coating film refers to the brightness measured in accordance with the provisions of JIS K5600-4-3.
[0108] The above-mentioned sparkle intensity (Si) and sparkle area (Sa value) are the following numerical values, namely: the coating is irradiated with an LED light source at an incident angle of 45°, an image is acquired using a CCD chip arranged perpendicularly to the coating, the acquired image is analyzed using an image analysis algorithm using a histogram of brightness levels, and a two-dimensional analysis is performed to calculate the brightness parameters, which are expressed as values of sparkle intensity (Sparkle intensity = Si value) and sparkle area (Sparkle area = Sa value).
[0109] By setting the gloss intensity (Si) of the cured coating film to a value of 5 or more and the gloss area (Sa value) to a value of 10 or more, it is shown that when a cured coating film is formed using a coating composition containing a coating film-forming resin and a flaky pigment, a coating film having higher brightness than conventional coating films can be formed.
[0110] The value of the brightness intensity (Si) is preferably 5 to 50, more preferably 6 to 40. The brightness area (Sa value) is preferably 10 to 60, more preferably 10 to 40.
[0111] The granularity value (G value) is a value obtained by measuring the granularity in a numerical manner by diffuse illumination. The granularity value (G value) is obtained by obtaining an image through a CCD chip under diffuse illumination in a hemisphere coated with white, analyzing the obtained image using a histogram of brightness levels, and showing the uniformity of the light and dark areas as a value representing 1 granularity. The granularity value (G value) is expressed in a range of 0 to 30, with smaller values indicating finer and larger values indicating more granular.
[0112] By setting the granularity value (G value) of the cured coating film to be 5 or more and 10 or less, when a cured coating film is formed using a coating composition containing a coating film-forming resin and a flaky pigment, it is possible to form a coating film having a high granularity and a unique design compared to conventional coating films.
[0113] The above-mentioned gloss intensity (Si), gloss area (Sa value), and granularity value (G value) can be measured using a gloss meter. Examples of the gloss meter capable of measuring these include BYK-mac (manufactured by BYK).
[0114] In the present disclosure, the chroma C* at an incident angle of 45° and a light receiving angle of 45° in the cured coating of the coating composition is 5 or less. Specifically, the light receiving angle refers to the light receiving angle at a position of 45° from the regular reflection light of light irradiated at an angle of 45° to the cured coating, i.e., a position perpendicular to the cured coating, from the regular reflection light to the incident angle direction, i.e., the position of the regular reflection light at 0°.
[0115] The above-mentioned chroma C* is a parameter in the L*C*h color system and can be obtained according to JIS Z8729. The L*C*h color system is a color system stipulated by the International Commission on Illumination and is recorded in Section 4.2 of CIE Publication 15.2 (1986). In the L*C*h color system, L* represents brightness, C* represents chroma, and h represents hue angle. Chroma C* means that as its value increases, the brightness of the measured substance increases, and as its value decreases, the dullness increases. The above-mentioned chroma C* can be measured using a commercially available multi-angle spectrophotometer. As a multi-angle spectrophotometer, for example, MA-68II (manufactured by X-Rite Co., Ltd.) and the like can be cited.
[0116] The angular flop value of the cured coating film of the above-mentioned coating composition is preferably 1.1 or more and less than 2. In this specification, the angular flop value (sometimes also described as FF value) is a value indicating the degree of change in the intensity of reflected light corresponding to the observation angle (light acceptance angle). The FF value is calculated by measuring the L* value at a light acceptance angle of 15 degrees (L* (15°) value) and the L* value at a light acceptance angle of 110 degrees (L* (110°) value) and using the following formula.
[0117] FF value = L*(15°) value / L*(110°) value
[0118] It should be noted that the L* value at the receiving angle of 15 degrees (L*(15°) value) is specifically the L* value of light received at a position of 15 degrees from the regular reflection angle relative to the incident angle in the direction of the measuring light when the measuring light is irradiated at an angle of 45 degrees relative to the axis perpendicular to the measuring object surface (incident angle 45 degrees). In addition, the L* value at the receiving angle of 110 degrees (L*(110°) value) is similarly the L* value of light received at an angle of 110 degrees from the regular reflection angle in the direction of the measuring light when the measuring light is irradiated.
[0119] The L* value at an acceptance angle of 15 degrees (L*(15°) value) and the L* value at an acceptance angle of 110 degrees (L*(110°) value) can be measured using a commercially available multi-angle spectrophotometer.
[0120] The larger the FF value, the larger the change in the L* value (brightness) caused by the observation angle (light receiving angle), and when the FF value is small, the change in the L* value (brightness) caused by the observation angle (light receiving angle) is small. In general metal coatings, when the FF value is large and the brightness change caused by the observation angle is large, the shadow sense of the metal coating is high, which is mostly used as a design target. On the other hand, the coating of the present invention is characterized in that it has a bright feeling as a whole coating, and on the other hand, it can also visually recognize the granular feeling that presents a bright feeling, and then it can also visually recognize the light color tone, which is a unique design. In such a coating of the present invention, due to the characteristic of visually recognizing the light color tone, the FF value becomes a significantly small value compared with general metal coatings. The above-mentioned FF value is more preferably 1.2 or more and less than 2, and is further preferably 1.2 or more and 1.8 or less.
[0121] The coating film disclosed in the present invention has the following characteristics: it has high brightness and a large bright area, and the coating film as a whole has a glossy feeling. On the other hand, a granular feeling and a light color tone that present a glossy feeling can also be visually recognized. The above-mentioned coating film has a glossy feeling as a whole due to these characteristics. On the other hand, a granular feeling that presents a glossy feeling can also be visually recognized, and a light color tone can also be visually recognized, which can present a unique design. In more detail, by using the coating composition disclosed in the present invention, in a coating film with a light color tone with a low chroma C* of less than 5, a coating film with a high granularity value G value of 5 to 10, which has both a light color tone and brightness and has a unique design can be formed.
[0122] Example
[0123] Hereinafter, the present invention will be described in detail with reference to specific examples, but the present invention is not limited to the following examples. In the examples, "parts" and "%" are based on mass unless otherwise specified.
[0124] Production Example 1: Production of acrylic resin emulsion (film-forming resin)
[0125] 633 parts of deionized water were placed in a reaction container, and the temperature was raised to 80° C. while mixing and stirring in a nitrogen stream. Next, 75.65 parts by mass of styrene (ST), 178.96 parts by mass of methyl methacrylate (MMA), 75.94 parts by mass of n-butyl acrylate (BA), 64.45 parts by mass of 2-ethylhexyl acrylate (2-EHA), 105.00 parts by mass of hydroxyethyl methacrylate (HEMA), a monomer emulsion consisting of 25.00 parts of Aqualon HS-10 (polyoxyethylene alkyl propylene phenyl ether sulfate, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), 25.00 parts of ADEKA RIASOAP NE-20 (α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxyethylene oxide, manufactured by Asahi Denka Co., Ltd.), and 400 parts of deionized water, and an initiator solution consisting of 1.2 parts of ammonium persulfate and 500 parts of deionized water were simultaneously added dropwise to the reaction container over 1.5 hours. After the addition was completed, aging was performed at the same temperature for 1 hour.
[0126] Furthermore, 53.65 parts by mass of styrene (ST), 178.96 parts by mass of methyl methacrylate (MMA), 75.94 parts by mass of n-butyl acrylate (BA), 64.45 parts by mass of 2-ethylhexyl acrylate (2-EHA), 105.00 parts by mass of hydroxyethyl methacrylate (HEMA), 22 parts by mass of acrylic acid, an emulsion of monomers consisting of 10 parts of Aqualon HS-10 and 250 parts of deionized water, and an initiator solution consisting of 3.0 parts of ammonium persulfate and 500 parts of deionized water were simultaneously added dropwise to the reaction container over 1.5 hours at 80° C. After the addition was completed, aging was performed at the same temperature for 2 hours.
[0127] Next, the mixture was cooled to 40°C, filtered through a 400-mesh filter, and 100 parts of deionized water and 1.6 parts of dimethylaminoethanol were added to adjust the pH to 6.5 to obtain an acrylic resin emulsion with an average particle size of 150 nm, a non-volatile component of 35%, a solid acid value of 20 mgKOH / g, and a hydroxyl value of 100 mgKOH / g.
[0128] Preparation Example 2: Preparation of an organic compound containing a phosphoric acid group
[0129] 40 parts of ethoxypropanol were placed in a 1-liter reaction container equipped with a stirrer, a temperature regulator, and a cooling tube, and 40 parts of a solution of 20 parts of Phosmer PP (acid phosphoryloxyhexa(oxypropylene)monomethacrylate manufactured by UniChemical) dissolved in 20 parts of ethoxypropanol, and 121.7 parts of a monomer solution consisting of 1.7 parts of azobisisobutyronitrile were added dropwise thereto at 120° C. for 3 hours, and then stirring was continued for another hour. The obtained phosphoric acid group-containing organic compound had an acid value of 105 mgKOH / g, a phosphoric acid group value of 55 mgKOH / g, a hydroxyl value of 60 mgKOH / g, a number average molecular weight of 6000, and a non-volatile content of 63%.
[0130] It should be noted that in the examples of this specification, the number average molecular weight is measured using "HLC8220GPC" (trade name, manufactured by Tosoh Corporation) as the GPC apparatus, using 4 "Shodex KF-606M" and "Shodex KF-603" (both trade names, manufactured by Showa Denko K.K.) as columns, under the conditions of mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 0.6cc / min, detector: RI.
[0131] In the examples of this specification, the acid value of the organic compound containing a phosphoric acid group and the phosphoric acid group value are calculated based on the definition of the acid value in JIS K5601.2-1 (the number of mg of potassium hydroxide (KOH) required to neutralize the free acid in 1 g of the sample (non-volatile matter)). In addition, the hydroxyl value is calculated based on the definition of the hydroxyl value in JIS K0070 (the number of mg of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of the sample is acetylated).
[0132] Example 1: Preparation of waterborne coating composition
[0133] 182 parts of the acrylic resin emulsion of Preparation Example 1, 2.2 parts of dimethylaminoethanol, 40 parts of CYMEL 327 (mixed alkylated melamine resin, manufactured by Allnex, solid content 90%), and Elgee neo Extra 10 parts (10 parts by mass relative to 100 parts by mass of resin solid content) of White#325 (flaky vapor-deposited metal pigment, manufactured by Oike Industry Co., Ltd., with an average particle size (average major diameter) of 35 μm and an active ingredient of 100%), 5 parts of the phosphoric acid group-containing organic compound of Preparation Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts (3 parts in terms of solid content) of Noigen EA-207D (amphiphilic compound, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., with a number average molecular weight of 4200 and a solid content of 55%), and 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed, dimethylaminoethanol was added in such a way that the pH became 8.1, and the mixture was diluted with deionized water to prepare an aqueous coating composition having a resin solid content concentration of 33% by mass.
[0134] Example 2: Preparation of waterborne coating composition
[0135] A water-based coating composition was prepared by the same procedure as in Example 1 except that the amount of Elgee neo Extra White #325 was changed to 40 parts (40 parts by mass relative to 100 parts by mass of the resin solid content).
[0136] Example 3: Preparation of waterborne coating composition
[0137] A water-based coating composition was prepared by the same procedure as in Example 1 except that 40 parts of Elgee neo Extra White #325 and 0.5 parts of fine-particle titanium oxide (MT-700HD, Tayca Corporation) were used.
[0138] Comparative Example 1: Preparation of water-based coating composition
[0139] A water-based coating composition was prepared by the same procedure as in Example 1 except that aluminum paste 01-0651 (a crushed aluminum bright pigment, manufactured by Toyo Aluminum Co., Ltd., active ingredient 61%, crushed aluminum pigment) was used in an amount of 9 parts by mass based on 100 parts by mass of the resin solid content instead of Elgee neo Extra White #325.
[0140] Comparative Example 2: Preparation of water-based coating composition
[0141] A water-based coating composition was prepared by the same procedure as in Example 1 except that 8 parts of aluminum paste 01-0651 (a crushed aluminum bright pigment, manufactured by Toyo Aluminum Co., Ltd., with an active ingredient of 61%, a crushed aluminum pigment) and 11 parts of fine-particle titanium oxide (MT-700HD, Tayca Co., Ltd.) were used relative to 100 parts by mass of the resin solid content instead of Elgee neo Extra White #325.
[0142] The following evaluations were performed using the aqueous coating compositions prepared in the above Examples and Comparative Examples. The evaluation results are shown in the following table.
[0143] Preparation of coating test panels
[0144] A zinc phosphate treated rough steel plate having a thickness of 0.8 mm, a length of 30 cm, and a width of 40 cm was electro-deposited with "Power top U-50" (manufactured by NIPPONPAINT AUTOMOTIVE COATINGS CO., LTD.) as a cationic electrodeposition coating composition in a dry film thickness of 20 μm, and the coated plate was sintered at 160° C. for 30 minutes. Then, a mid-coat coating composition "OP-30P middle gray" (manufactured by NIPPON PAINT AUTOMOTIVE COATINGS CO., LTD., a polyester melamine-based paint, pre-diluted for 25 seconds (measured at 20° C. using a No. 4 Ford cup) was pneumatically atomized and then cured by sintering at 140° C. for 30 minutes to form a cured mid-coat coating film having a brightness of 60.
[0145] Next, the water-based coating composition prepared in the examples or comparative examples was applied by pneumatic atomization at room temperature of 23° C. and humidity of 68% to a dry film thickness of 15 μm. After 4 minutes of standing, it was preheated at 80° C. for 5 minutes.
[0146] After preheating, the coated plate was cooled to room temperature, and a clear coating of MACFLOW-O-1810 (solvent-based clear coating manufactured by NIPPON PAINTAUTOMOTIVE COATINGS CO., LTD.) was applied by pneumatic atomization for 7 minutes in a manner such that the dry film thickness was 35 μm. Next, the coated plate was sintered at 140° C. for 30 minutes in a dryer to obtain a coated test plate having a multilayer coating film.
[0147] Determination of brightness intensity (Si), brightness area (Sa value) and granularity value (G value)
[0148] The obtained painted test plate was used to measure the glossiness using BYK-mac i (multi-angle (6-angle) colorimetry, glossiness / particle measurement instrument) manufactured by BYK to determine the glossiness intensity (Si) and glossiness area (Sa value) at an incident angle of 45°.
[0149] Determination of chroma C*
[0150] The obtained painted test plate was used to measure the chromaticity C* at an incident angle of 45° and a light receiving angle of 45° using a multi-angle spectrophotometer MA-68II (manufactured by X-Rite Corporation).
[0151] Determination of FF value
[0152] For the obtained painted test plate, the L* value at an incident angle of 45 degrees and an acceptance angle of 15 degrees (L*(15°) value) and the L* value at an acceptance angle of 110 degrees (L*(110°) value) were measured using a multi-angle spectrophotometer MA-68II (trade name, manufactured by X-Rite Corporation), and the FF value was calculated by the following formula.
[0153] FF value = L*(15°) value / L*(110°) value)
[0154] [Table 1]
[0155] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Brightness intensity (Si) 9.3 8.7 6.9 7.0 6.7 Brightness area (Sa) 27.1 30.3 26.6 21.1 23.1 Granularity value (G value) 9.1 8.6 6.0 4.8 4.0 Chroma C* 2.6 1.6 1.6 2.1 4.8 L*(15°) value 84.4 93.8 96.9 111.1 114.9 L*(110°) value 58.5 56.9 67.0 26.3 51.2 FF value (L*15° / 110°) 1.4 1.6 1.4 4.2 2.2
[0156] The coating film formed using the coating composition of the example has high gloss intensity (Si), gloss area (Sa value) and granularity value (Ga value), and the coating film as a whole has a glossy feeling, and on the other hand, a granular feeling showing a glossy feeling can also be visually recognized. Furthermore, a light color tone is observed from the coating film.
[0157] Comparative Example 1 is an example using a crushed aluminum pigment. In this example, it was confirmed that the gloss intensity (Si) and gloss area (Sa value) were high, and the coating film as a whole had a glossy feel, while the granularity value was low, and the granularity that showed the glossy feel was low.
[0158] Comparative Example 2 is an example using a crushed aluminum pigment and a white pigment (micro-particle titanium oxide). In this example, by containing a white pigment, a light color tone is visually recognized from the coating film. In addition, the gloss intensity (Si) and the gloss area (Sa value) are high, and the coating film as a whole has a glossy feel. On the other hand, it is confirmed that the granularity value is low, and the granularity that presents a glossy feel is low.
[0159] Industrial Applicability
[0160] The coating film formed by using the coating composition of the present disclosure has the following unique design: high brightness and a large bright area, the coating film as a whole has a glossy feeling, and on the other hand, the glossy granular feeling and light color tone can also be visually recognized. The above-mentioned coating film can be suitably used as a design coating film for various articles.
Claims
1. A coating composition comprising a coating film-forming resin, an organic compound containing a phosphoric acid group and a pigment, The coating film forming resin comprises acrylic resin, polyester resin, polyurethane resin, epoxy resin, fluororesin or silicone resin. The pigment comprises a flaky vapor-deposited metal pigment, the flaky vapor-deposited metal pigment comprises a first protective layer, a vapor-deposited metal layer, and a second protective layer in this order, the aspect ratio of the flaky vapor-deposited metal pigment is 5 to 50, the first protective layer and the second protective layer each comprise an organic silicon component, the vapor-deposited metal layer comprises aluminum, copper, gold, silver, zinc, titanium, chromium, nickel, nickel-chromium, stainless steel, a mixture thereof, or an alloy thereof, and the amount of the flaky vapor-deposited metal pigment contained in the coating composition is in the range of 0.1 to 40 parts by mass relative to 100 parts by mass of the resin solid content of the coating film forming resin, The cured coating film of the coating composition has a luminous intensity (Si) of 5 or more at an incident angle of 45°, a luminous area (Sa) of 10 or more, and a granularity value (G) of 5 or more and 10 or less. The chromaticity C* is less than 5 when the incident angle is 45° and the receiving angle is 45°. The cured coating film has a color flop value of 1.1 or more and less than 2.
2. The coating composition according to claim 1, wherein The average particle size of the flaky vapor-deposited metal pigment is 10-150 μm, and the average thickness is 0.5-10 μm.
3. The coating composition according to claim 2, wherein The average thickness of each layer of the first protective layer and the second protective layer is 0.5-3 μm, The average thickness of the evaporated metal layer is 5-100 nm.
4. The coating composition according to claim 2, wherein The evaporated metal layer includes aluminum.
5. A method for producing a cured coating film, comprising the steps of applying the coating composition according to any one of claims 1 to 4 to an object to be coated, and then heating and curing the object. The cured coating film has a luminous intensity Si of 5 or more at an incident angle of 45°, a luminous area Sa of 10 or more, a granularity G of 5 or more and 10 or less, and a chromaticity C* of 5 or less at an incident angle of 45° and a light receiving angle of 45°. The cured coating film has a color flop value of 1.1 or more and less than 2. 6 . An article comprising a cured coating film of the coating composition according to claim 1 .
Citation Information
Patent Citations
Coating composition, coated article and method for forming multilayer coating film
WO2019131957A1
Multi-layered coating film formation method
JP2017159217A