Ultrafiltration membrane with electrocatalytic function and preparation method and application thereof
By introducing a polydopamine mediating layer and a conductive polymer polyaniline into the ultrafiltration membrane, an ultrafiltration membrane with electrocatalytic function is formed, which solves the problems of poor anti-pollution ability and high production cost of the existing ultrafiltration membrane, and achieves a more efficient Decomposition of organic contaminants and long-life membrane performance.
Patent Information
- Application Number
- CN202111069258.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-13
Smart Images

Figure BDA0003259849490000101 
Figure BDA0003259849490000102 
Figure BDA0003259849490000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultrafiltration, and in particular to an ultrafiltration membrane with electrocatalytic function and a preparation method and application thereof. Background Art
[0002] Ultrafiltration technology plays an important role in reverse osmosis pretreatment, drinking water purification, deep treatment and reuse of domestic sewage and industrial wastewater, clarification of fruit juice drinks, alcoholic beverages and pharmaceutical preparations, concentration and purification of biological products. However, membrane pollution has always been a serious problem faced by the promotion and application of ultrafiltration technology. Membrane pollution will not only cause a decrease in flux, but also increase operating costs and shorten the service life of the membrane. In severe cases, it will cause the membrane pores to be blocked, causing the entire membrane system to fail to work. Membrane pollutants mainly include inorganic pollutants and organic pollutants. Among them, organic pollutants have a strong force on the membrane surface, and it is difficult to remove them by conventional pure water mechanical cleaning. The chemical agent flushing method not only has high requirements on the strength of the membrane, but also may cause environmental pollution.
[0003] Electrocatalytic oxidation technology is to react at the anode of the electrode through an external electric field. In this process, organic matter can be directly degraded, or substances with strong oxidizing properties (such as hydroxyl radicals, superoxide anion radicals, etc.) can be produced to react with organic pollutants to decompose them into small molecular organic matter or directly degrade them into water and carbon dioxide. This method is simple and efficient, without secondary pollution, and is called "environmentally friendly technology". Combining ultrafiltration technology with electrocatalytic oxidation technology, the ultrafiltration membrane can not only be used as a carrier of electrocatalysts to degrade pollutants through electrocatalytic oxidation, but also as a separation barrier for degradation products. At present, most electrocatalytic filtration membranes are prepared by coating materials with electrocatalytic functions on the surface of the base membrane. However, this method has the problem of weak bonding between the electrocatalytic functional layer and the base membrane, which shortens the service life of the catalytic membrane. In addition, since most polymer membrane materials do not have conductivity and cannot be directly applied to the electrocatalytic process, the commonly used method is to use carbon nanotubes, graphene, etc. with good conductivity to enhance the conductivity of the membrane, but this will increase the production cost. Summary of the invention
[0004] Aiming at the problems of poor anti-pollution ability of ultrafiltration membranes in the prior art, complicated production process, high production cost, etc., the present invention proposes an ultrafiltration membrane with electrocatalytic function and a preparation method and application thereof.
[0005] In order to achieve the above-mentioned objectives, the first aspect of the present invention provides a method for preparing an ultrafiltration membrane with electrocatalytic function, the method comprising mixing a catalyst containing a polydopamine mediating layer with a casting liquid containing polyaniline to obtain a blended casting liquid, and then coating the blended casting liquid onto a conductive support layer.
[0006] The second aspect of the present invention provides an ultrafiltration membrane with electrocatalytic function prepared by the above method.
[0007] The third aspect of the present invention provides an ultrafiltration membrane with electrocatalytic function, the ultrafiltration membrane comprising a conductive support layer and a membrane layer supported on the conductive support layer, the membrane layer containing polyaniline and a catalyst having a polydopamine mediating layer.
[0008] A fourth aspect of the present invention provides the use of the ultrafiltration membrane described above in wastewater treatment and / or degradation of organic pollutants.
[0009] The present invention introduces a polydopamine mediating layer on the catalyst surface on the one hand, and uses a conductive support layer and introduces conductive polymer polyaniline on the other hand, thereby obtaining an ultrafiltration membrane with enhanced bonding between the catalyst and the membrane layer and improved conductivity. Under the action of an electric field, the catalyst in the ultrafiltration membrane electrolyzes water to produce strong oxidants such as hydroxyl radicals, which decompose the organic pollutants that are difficult to degrade on the surface of the ultrafiltration membrane into small molecular organic matter or carbon dioxide and water. The method makes the decomposition of organic matter more thorough, is not easy to produce secondary pollutants, and significantly improves the anti-pollution ability of the ultrafiltration membrane, showing good potential in preparing an ultrafiltration membrane with long-term stable anti-pollution performance. The method of the present invention is simple to operate, the preparation process is environmentally friendly, and the raw materials are easily available, which is suitable for industrial production. DETAILED DESCRIPTION
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0011] The first aspect of the present invention provides a method for preparing an ultrafiltration membrane with electrocatalytic function, the method comprising mixing a catalyst containing a polydopamine mediating layer with a casting liquid containing polyaniline to obtain a blended casting liquid, and then coating the blended casting liquid onto a conductive support layer.
[0012] According to the present invention, in order to enhance the bonding force between the catalyst and the membrane, preferably, the catalyst containing the polydopamine mediation layer is obtained by the following method: a transition metal catalyst is contacted with a dopamine hydrochloride solution at 10-40° C. for 0.5-5 hours. The transition metal catalyst is reacted with dopamine hydrochloride to construct a polydopamine mediation layer having -NH2 active sites on the catalyst surface.
[0013] According to the present invention, the amount of the transition metal catalyst and the dopamine hydrochloride solution can be selected within a wide range. Preferably, the mass volume ratio of the transition metal catalyst to the dopamine hydrochloride solution is (3-10) g:100 mL.
[0014] According to the present invention, preferably, the concentration of the dopamine hydrochloride solution is 0.5-5 g / L.
[0015] According to the present invention, in order to enable dopamine to better modify the catalyst and construct a polydopamine mediation layer with -NH2 active sites on the catalyst surface, preferably, the dopamine hydrochloride solution is prepared by the following method: first prepare a tris buffer solution, then use HCl to adjust the pH value of the solution, and after adjusting the pH value to 7-9, add dopamine hydrochloride powder so that the concentration of the dopamine hydrochloride solution is 0.5-5g / L.
[0016] According to the present invention, the transition metal catalyst may be a catalyst commonly used for degrading organic pollutants. Preferably, the transition metal catalyst comprises a transition metal oxide catalyst and / or a transition metal sulfide catalyst. More preferably, the transition metal oxide catalyst is selected from at least one of titanium dioxide, ferric oxide, manganese dioxide and ferrosoferric oxide; more preferably, the transition metal sulfide catalyst is cadmium sulfide.
[0017] According to the present invention, preferably, the particle size of the transition metal catalyst is 3-10 nm. "Particle size" refers to "average particle size" or "particle size distribution range".
[0018] According to the present invention, preferably, the polyaniline-containing casting solution comprises 10-20 wt % of membrane material, 0.5-5 wt % of polyaniline, 1-10 wt % of additives and 65-85 wt % of solvent.
[0019] According to the present invention, the membrane material is a commonly used membrane material in the art, preferably, the membrane material includes polysulfones and / or fluorine-containing polymers, more preferably, the polysulfones are polyethersulfones, and the fluorine-containing polymers are polyvinylidene fluoride. The weight average molecular weight of the polyvinylidene fluoride is distributed between 300,000 and 450,000, and the weight average molecular weight of the polyethersulfone is distributed between 40,000 and 60,000.
[0020] According to the present invention, preferably, the additive includes an inorganic additive and / or an organic additive, more preferably, the inorganic additive includes at least one of sodium chloride, lithium chloride, calcium chloride, lithium nitrate, calcium nitrate, magnesium chloride and zinc chloride, more preferably, the organic additive includes at least one of polyethylene glycol (the average molecular weight of polyethylene glycol is 200-600, preferably 380-400), ethyl acetate, polymaleic anhydride, cyclohexanol, glycerol, triethyl phosphate, tributyl phosphate and polyvinyl pyrrolidone (the weight average molecular weight of polyvinyl pyrrolidone is distributed between 44000 and 54000). The introduction of the above additives can improve the interaction of the components in the casting solution, reduce the solvation in the original polymer solution, and effectively adjust the pore size, porosity, hydrophilicity, etc. of the membrane.
[0021] According to the present invention, preferably, the solvent includes at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.
[0022] According to the present invention, preferably, the blended casting solution is prepared by the following method: heating the casting solution containing polyaniline to 30-80° C., mixing it with a catalyst containing a polydopamine mediating layer, and ultrasonically treating it for 2-4 hours.
[0023] According to the present invention, preferably, the ultrasonic treatment is followed by standing for 12-24 hours for defoaming.
[0024] According to the present invention, preferably, the weight content of the catalyst containing the polydopamine mediating layer in the blended casting solution is 1-15 weight %, preferably 4-10 weight %.
[0025] According to the present invention, the conductive support layer may be a material having conductive properties. In order to reduce the production cost of the ultrafiltration membrane, preferably, the conductive support layer is a carbon fiber cloth.
[0026] According to the present invention, preferably, the conductive support layer has a thickness of 100-300 μm and a gram weight of 200 g / m 2 -280g / m 2 .
[0027] According to the present invention, preferably, the method for preparing an ultrafiltration membrane with an electrocatalytic function further comprises applying the blended casting liquid to the conductive support layer and then placing it in a coagulation bath for curing, and then sequentially performing a desolventizing treatment, a pore preservation treatment and drying. The pore preservation treatment and drying are both commonly used conditions in the art, preferably, immersing in a 0.2wt% sodium dodecyl sulfate solution for 5-6 days, and then drying at a humidity of 88% and 20-30°C.
[0028] According to the present invention, preferably, the bath liquid used in the coagulation bath is water.
[0029] According to the present invention, preferably, the curing temperature is 20-60°C.
[0030] According to the present invention, preferably, the desolventizing treatment time is 24-72 hours.
[0031] The second aspect of the present invention provides an ultrafiltration membrane with electrocatalytic function prepared by the above method.
[0032] The third aspect of the present invention provides an ultrafiltration membrane with electrocatalytic function, the ultrafiltration membrane comprising a conductive support layer and a membrane layer supported on the conductive support layer, the membrane layer containing polyaniline and a catalyst having a polydopamine mediating layer.
[0033] According to the present invention, preferably, the thickness of the film layer is 60 μm-80 μm.
[0034] According to the present invention, preferably, the catalyst in the catalyst containing the polydopamine mediation layer is a transition metal catalyst, more preferably, the transition metal catalyst includes a transition metal oxide catalyst and / or a transition metal sulfide catalyst; further preferably, the transition metal oxide catalyst is selected from at least one of titanium dioxide, ferric oxide, manganese dioxide and ferrosoferric oxide; further preferably, the transition metal sulfide catalyst is cadmium sulfide.
[0035] According to the present invention, preferably, the thickness of the conductive support layer is 100-300 μm, preferably 150 μm-200 μm.
[0036] According to the present invention, preferably, the conductive support layer is carbon fiber cloth.
[0037] According to the present invention, preferably, the membrane layer further contains polysulfones and / or fluorine-containing polymers, more preferably, the polysulfones are polyethersulfones, and the fluorine-containing polymers are polyvinylidene fluoride.
[0038] According to the present invention, preferably, the film layer also contains inorganic additives and / or organic additives. More preferably, the inorganic additives include at least one of sodium chloride, lithium chloride, calcium chloride, lithium nitrate, calcium nitrate, magnesium chloride and zinc chloride. More preferably, the organic additives include at least one of polyethylene glycol, ethyl acetate, polymaleic anhydride, cyclohexanol, glycerol, triethyl phosphate, tributyl phosphate and polyvinyl pyrrolidone.
[0039] A fourth aspect of the present invention provides the use of the ultrafiltration membrane described above in wastewater treatment and / or degradation of organic pollutants.
[0040] The present invention will be described in detail below by way of examples. In the following examples,
[0041] The average weight average molecular weight of polyaniline was 20,000.
[0042] The thickness of the carbon fiber cloth is 120μm and the weight is 200g / m 2 .
[0043] The weight average molecular weight of polyvinylidene fluoride is distributed between 300,000 and 450,000.
[0044] The average molecular weight of polyethylene glycol is 380-400.
[0045] The weight average molecular weight of polyethersulfone is distributed between 40,000 and 60,000.
[0046] The brand of polyvinyl pyrrolidone is PVP K30, and the weight average molecular weight is distributed between 44000 and 54000.
[0047] The pore-preserving treatment and drying conditions include soaking in a 0.2 wt % sodium dodecyl sulfate solution for 5-6 days and then drying at a humidity of 88% and 25° C.
[0048] Example 1
[0049] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0050] (1) Modification of the catalyst: First prepare a Tris-HCl buffer solution with a pH value of 8.5, then add dopamine hydrochloride powder to prepare a 5 g / L dopamine hydrochloride solution, soak 4 g of titanium dioxide (average particle size of 5 nm) in 100 mL of the 5 g / L dopamine hydrochloride solution, and stir at 30° C. for 2 hours to obtain a catalyst containing a polydopamine mediation layer.
[0051] (2) Preparation of blended casting solution: 15 g polyvinylidene fluoride, 1 g polyaniline, 5 g glycerol and 79 g N-methylpyrrolidone were mixed, heated to 80°C, and mixed evenly by mechanical stirring to obtain a preliminary casting solution. Then 4 g of the catalyst containing the polydopamine mediating layer was mixed with 96 g of the preliminary casting solution and ultrasonicated for 4 hours to disperse the catalyst evenly. After standing for 12 hours to defoam, a blended casting solution was obtained.
[0052] (3) Preparation of catalytic ultrafiltration membrane: The blended membrane casting liquid is evenly coated on the carbon fiber cloth with a scraper, and then it is placed in a deionized water coagulation bath and soaked until the liquid film is completely solidified and then taken out. The coagulation bath temperature is 60°C, and then the solidified membrane is soaked in deionized water for 72 hours for solvent removal treatment. After pore preservation treatment, it is dried to obtain an ultrafiltration membrane with electrocatalytic function.
[0053] Example 2
[0054] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0055] (1) Modification of the catalyst: First, prepare a Tris-HCl buffer solution with a pH value of 8, then add dopamine hydrochloride powder to prepare a 2 g / L dopamine hydrochloride solution, soak 8 g of cadmium sulfide (average particle size of 4 nm) in 100 mL of the 2 g / L dopamine hydrochloride solution, and stir at 25° C. for 3 hours to obtain a catalyst containing a polydopamine mediation layer.
[0056] (2) Preparation of blended casting solution: 15 g of polyvinylidene fluoride, 5 g of polyaniline, 5 g of polyethylene glycol and 75 g of dimethylformamide were mixed, heated to 60°C, and mixed evenly by mechanical stirring to obtain a preliminary casting solution. Then 5 g of the catalyst containing the polydopamine mediating layer was mixed with 95 g of the preliminary casting solution and ultrasonicated for 2 hours to disperse the catalyst evenly. After standing for 12 hours to defoam, a blended casting solution was obtained.
[0057] (3) Preparation of catalytic ultrafiltration membrane: The blended membrane casting liquid is evenly coated on the carbon fiber cloth with a scraper, and then it is placed in a deionized water coagulation bath and soaked until the liquid film is completely solidified and then taken out. The coagulation bath temperature is 40°C, and then the solidified membrane is soaked in deionized water for 48 hours for solvent removal treatment. After pore preservation treatment, it is dried to obtain the ultrafiltration membrane of the present invention.
[0058] Example 3
[0059] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0060] (1) Modification of the catalyst: First prepare a Tris-HCl buffer solution with a pH value of 7.5, then add dopamine hydrochloride powder to prepare a 0.5 g / L dopamine hydrochloride solution, soak 8 g of ferrosoferric oxide (average particle size of 10 nm) in 100 mL of the 0.5 g / L dopamine hydrochloride solution, and stir at 25° C. for 1 hour to obtain a catalyst containing a polydopamine mediation layer.
[0061] (2) Preparation of blended casting solution: 15 g polyethersulfone, 5 g polyaniline, 5 g lithium chloride and 75 g dimethyl sulfoxide were mixed, heated to 40°C, and mixed evenly by mechanical stirring to obtain a preliminary casting solution. Then 10 g of the catalyst containing the polydopamine mediating layer was mixed with 90 g of the preliminary casting solution and ultrasonicated for 2 hours to disperse the catalyst evenly. After standing for 24 hours to defoam, a blended casting solution was obtained.
[0062] (3) Preparation of catalytic ultrafiltration membrane: The blended membrane casting liquid is evenly coated on the carbon fiber cloth with a scraper, and then it is placed in a deionized water coagulation bath and soaked until the liquid film is completely solidified and then taken out. The coagulation bath temperature is 40°C, and then the solidified membrane is soaked in deionized water for 72 hours for solvent removal treatment. After pore preservation treatment, it is dried to obtain the ultrafiltration membrane of the present invention.
[0063] Example 4
[0064] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0065] (1) Modification of the catalyst: First prepare a Tris-HCl buffer solution with a pH value of 8.5, then add dopamine hydrochloride powder to prepare a 5 g / L dopamine hydrochloride solution, soak 3 g of titanium dioxide (average particle size of 10 nm) in 100 mL of the 5 g / L dopamine hydrochloride solution, and stir at 25°C for 1 hour to obtain a catalyst containing a polydopamine mediation layer.
[0066] (2) Preparation of blended casting solution: 18 g of polyethersulfone, 2 g of polyaniline, 5 g of polyvinylpyrrolidone and 75 g of dimethylacetamide were mixed, heated to 30°C, and mixed evenly by mechanical stirring to obtain a preliminary casting solution. Then 8 g of the catalyst containing the polydopamine mediating layer was mixed with 92 g of the preliminary casting solution and ultrasonicated for 2 hours to evenly disperse the catalyst. After standing for 24 hours to defoam, a blended casting solution was obtained.
[0067] (3) Preparation of catalytic ultrafiltration membrane: The blended membrane casting liquid is evenly coated on the carbon fiber cloth with a scraper, and then it is placed in a deionized water coagulation bath and soaked until the liquid film is completely solidified and then taken out. The coagulation bath temperature is 25°C, and then the solidified membrane is soaked in deionized water for 72 hours for solvent removal treatment. After pore preservation treatment, it is dried to obtain the ultrafiltration membrane of the present invention.
[0068] Example 5
[0069] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0070] The ultrafiltration membrane was prepared according to the method of Example 1, except that the amount of polyvinylidene fluoride used was 15 g, the amount of polyaniline used was 0.2 g, the amount of glycerol used was 5 g, and the amount of N-methylpyrrolidone used was 79.8 g.
[0071] Example 6
[0072] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0073] The ultrafiltration membrane was prepared according to the method of Example 1, except that 2 g of the catalyst containing the polydopamine mediating layer was mixed with 98 g of the preliminary membrane casting solution.
[0074] Comparative Example 1
[0075] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0076] The ultrafiltration membrane was prepared according to the method of Example 1, except that the carbon fiber cloth was replaced by a non-woven fabric (brand: TA3618, unit mass 125 g / m 2 , thickness 160μm).
[0077] Comparative Example 2
[0078] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0079] The ultrafiltration membrane was prepared according to the method of Example 1, except that no polyaniline was added and the amount of polyvinylidene fluoride used was 16 g.
[0080] Comparative Example 3
[0081] This example is used to illustrate the method for preparing an ultrafiltration membrane with electrocatalytic function
[0082] The ultrafiltration membrane was prepared according to the method of Example 1, except that no catalyst containing a polydopamine mediating layer was added.
[0083] Test Example 1
[0084] Anti-pollution performance test
[0085] The ultrafiltration membrane was placed in an existing wastewater treatment system, and BSA solution (BSA molecular weight of 67000, solution concentration of 0.1g / L) was added to the system as organic wastewater, and 5V DC was applied to the ultrafiltration membrane. After the system was run for 1 hour, the ultrafiltration membrane was taken out and soaked in distilled water for 2 hours. Then, the membrane flux was tested using a cup-type ultrafiltration system. High-purity nitrogen was used for pressure driving, and the driving pressure was 0.1MPa. The pure water flux J within 5 minutes was measured. W , the calculation formula of the water flux attenuation coefficient m is as follows:
[0086]
[0087] Where: m is the water flux attenuation coefficient, J0 is the initial water flux of the ultrafiltration membrane before wastewater treatment, J W is the water flux of the ultrafiltration membrane after wastewater treatment.
[0088] Table 1
[0089]
[0090]
[0091] It can be seen from the results in Table 1 that the embodiments 1 to 4 of the present invention have significantly better effects. The electrocatalytic ultrafiltration membrane prepared by the present invention can effectively reduce the water flux attenuation coefficient and improve the anti-pollution ability of the ultrafiltration membrane.
[0092] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing an ultrafiltration membrane with electrocatalytic function, characterized in that: The method comprises mixing a catalyst containing a polydopamine mediating layer with a casting solution containing polyaniline to obtain a blended casting solution, and then coating the blended casting solution onto a conductive support layer; The catalyst containing the polydopamine mediating layer is obtained by the following method: a transition metal catalyst is contacted with a dopamine hydrochloride solution at 10-40° C. for a reaction of 0.5-5 hours.
2. The method according to claim 1, wherein: The mass volume ratio of the transition metal catalyst to the dopamine hydrochloride solution is (3-10) g:100 mL.
3. The method according to claim 1, wherein: The concentration of the dopamine hydrochloride solution is 0.5-5 g / L.
4. The method according to claim 1, wherein: The transition metal catalyst includes a transition metal oxide catalyst and / or a transition metal sulfide catalyst.
5. The method according to claim 1, wherein: The particle size of the transition metal catalyst is 3-10 nm.
6. The method according to claim 4, wherein: The transition metal oxide catalyst is selected from at least one of titanium dioxide, ferric oxide, manganese dioxide and ferrosoferric oxide.
7. The method according to claim 4, wherein: The transition metal sulfide catalyst is cadmium sulfide.
8. The method according to claim 1, wherein: The polyaniline-containing casting solution comprises 10-20 weight percent of membrane material, 0.5-5 weight percent of polyaniline, 1-10 weight percent of additives and 65-85 weight percent of solvent.
9. The method according to claim 8, wherein: The membrane material includes polysulfones and / or fluorine-containing polymers.
10. The method according to claim 9, wherein: The polysulfone is polyethersulfone, and the fluorine-containing polymer is polyvinylidene fluoride.
11. The method according to claim 8, wherein: The additives include inorganic additives and / or organic additives.
12. The method according to claim 11, wherein: The inorganic additive includes at least one of sodium chloride, lithium chloride, calcium chloride, lithium nitrate, calcium nitrate, magnesium chloride and zinc chloride.
13. The method according to claim 11, wherein: The organic additive includes at least one of polyethylene glycol, ethyl acetate, polymaleic anhydride, cyclohexanol, glycerol, triethyl phosphate, tributyl phosphate and polyvinyl pyrrolidone.
14. The method according to claim 8, wherein: The solvent includes at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone.
15. The method according to claim 1, wherein: The blended casting solution is prepared by the following method: the casting solution containing polyaniline is heated to 30-80° C., mixed with a catalyst containing a polydopamine mediating layer, and subjected to ultrasonic treatment for 2-4 hours.
16. The method according to claim 1, wherein: The weight content of the catalyst containing the polydopamine mediating layer in the blended casting solution is 1-15 weight %.
17. The method according to claim 1, wherein: The weight content of the catalyst containing the polydopamine mediating layer in the blended casting solution is 4-10 weight %.
18. The method according to claim 1, wherein: The conductive support layer is carbon fiber cloth; And / or, the thickness of the conductive support layer is 100 μm-300 μm, and the weight is 200 g / m 2 -280g / m 2 .
19. The method according to claim 1, wherein: The method for preparing an ultrafiltration membrane with an electrocatalytic function also includes coating the blended membrane casting liquid onto a conductive support layer and then placing the mixture in a coagulation bath for solidification, and then sequentially performing a solvent removal treatment, a pore preservation treatment and drying.
20. The method according to claim 19, wherein: The bath liquid used in the coagulation bath is water.
21. The method according to claim 19, wherein: The curing temperature is 20-60°C.
22. The method according to claim 19, wherein: The desolventizing treatment time is 24-72h.
23. An ultrafiltration membrane with electrocatalytic function prepared by the method according to any one of claims 1 to 22.
24. An ultrafiltration membrane with electrocatalytic function, characterized in that: The ultrafiltration membrane comprises a conductive support layer and a membrane layer supported on the conductive support layer, wherein the membrane layer contains polyaniline and a catalyst having a polydopamine mediating layer; The catalyst containing the polydopamine mediating layer is obtained by the following method: a transition metal catalyst is contacted with a dopamine hydrochloride solution at 10-40° C. for reaction for 0.5-5 hours.
25. The ultrafiltration membrane according to claim 24, wherein The thickness of the film layer is 60 μm-80 μm.
26. The ultrafiltration membrane according to claim 24, wherein The transition metal catalyst includes a transition metal oxide catalyst and / or a transition metal sulfide catalyst.
27. The ultrafiltration membrane according to claim 24, wherein The thickness of the conductive support layer is 100 μm-300 μm.
28. The ultrafiltration membrane according to claim 24, wherein The conductive support layer is carbon fiber cloth.
29. The ultrafiltration membrane according to claim 24, wherein The membrane layer also contains polysulfones and / or fluorine-containing polymers.
30. The ultrafiltration membrane according to claim 24, wherein The film layer also contains inorganic additives and / or organic additives.
31. The ultrafiltration membrane according to claim 24, wherein The thickness of the conductive support layer is 150 μm-200 μm.
32. The ultrafiltration membrane according to claim 29, wherein The polysulfone is polyethersulfone, and the fluorine-containing polymer is polyvinylidene fluoride.
33. The ultrafiltration membrane according to claim 30, wherein The inorganic additive includes at least one of sodium chloride, lithium chloride, calcium chloride, lithium nitrate, calcium nitrate, magnesium chloride and zinc chloride.
34. The ultrafiltration membrane according to claim 30, wherein The organic additives include polyethylene At least one of glycol, ethyl acetate, polymaleic anhydride, cyclohexanol, glycerol, triethyl phosphate, tributyl phosphate and polyvinyl pyrrolidone.
35. Use of the ultrafiltration membrane according to any one of claims 24 to 34 in wastewater treatment and / or degradation of organic pollutants.