A chemically silver-plated slurry for low-temperature co-fired ceramics and a preparation method thereof

By using specific compositional liquid-plating silver paste in low-temperature co-fired ceramic process, the problem of mismatch between silver paste and raw ceramic sintering is solved, the stability of the substrate and the acid resistance of the silver layer are achieved, and it is suitable for all Silver plating processing avoids substrate deformation and improves gold wire bonding strength.

CN115810438BActive Publication Date: 2024-11-15NO 43 INST OF CHINA ELECTRONICS TECH GRP CETC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211475021.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-11-15
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

In the existing low-temperature co-fired ceramic process, the sintering between silver paste and raw ceramics does not match, resulting in deformation or warping of the substrate. In addition, traditional silver conductors are unstable in the electroless nickel/gold process, making it difficult to achieve full silver plating. Processing.

Method used

Using an immersible silver plating paste composed of 70-90 wt% silver powder, 0.1-7 wt% inorganic glass powder and organic carrier, the combination of the specific composition of inorganic glass powder and organic carrier is used to control the slurry and raw porcelain. The sintering matching properties and the fineness of screen printing is achieved through multiple rolling, and the submerged silver-plating paste is prepared.

Benefits of technology

The sintering shrinkage consistency between the silver-based layer and the LTCC substrate is achieved, which avoids the warping and deformation of the substrate. At the same time, the acid resistance and water resistance of the silver-based layer are improved, adapted to the electroless nickel/gold process, and ensured the silver conductor film layer. stability and gold wire bond strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115810438B_ABST
    Figure CN115810438B_ABST
Patent Text Reader

Abstract

The invention discloses a chemically silver-plated slurry for low-temperature co-fired ceramics and a preparation method thereof. The chemically silver-plated slurry is rolled from 70-90wt% of silver powder, 0.1-7wt% of inorganic glass powder and the remainder of an organic carrier; wherein the inorganic glass powder is composed of B2O3, SiO2, SrO, BaO, ZnO, Al2O3, TiO2, K2O, MgO, SnO2 and ZrO2. The inorganic glass powder of a specific composition is used. On the one hand, the sintering matching between the glass powder and the raw ceramic is controlled to meet the low-temperature co-fired ceramic process conditions, so that the chemically silver-plated slurry has good consistency with the sintering shrinkage rate of the LTCC substrate, and will not cause warping or deformation of the substrate; on the other hand, the bonding force between the slurry and the ceramic is increased, and the acid resistance and water resistance of the metallized silver layer are improved to adapt to the chemical nickel / gold plating process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a chemically plating silver paste for low temperature co-fired ceramics and a preparation method thereof. Background Art

[0002] With the rapid development of microelectronic information technology, electronic components are gradually moving towards lightweight, miniaturization, multifunctionality, high reliability and high integration, which puts forward higher requirements for microelectronic packaging technology. Low temperature co-fired ceramic technology (LTCC) has been widely used in SIP and high-frequency microwave components. LTCC substrate, as a high-density distribution carrier, undertakes the function of signal transmission. Active devices and passive devices such as capacitors, inductors and filters are mounted on the surface of LTCC substrate to realize component functions.

[0003] At present, the pastes used in the processing and production of LTCC substrates are mostly gold paste and silver-palladium paste. In order to reduce the processing and production costs of LTCC, it is possible to use silver conductor wiring. Traditional silver conductors are not as stable as gold conductors, so the use of full silver chemical plating becomes possible. Currently, there is little research on chemically plated silver paste on the market. It is urgent to develop a chemically plated silver paste to reduce the processing and production costs of LTCC. The chemically plated silver paste can be matched and co-fired with green porcelain to ensure that the sintering of the paste is consistent with the sintering of the green porcelain.

[0004] In addition, the current silver paste mostly solves the acid resistance problem of the paste in the ceramic post-firing process, but the shrinkage mismatch problem between the paste and the green ceramic in the low-temperature co-fired ceramic process has not been solved, which is very likely to cause deformation or warping of the substrate. Summary of the invention

[0005] In view of this, it is necessary for the present invention to provide a chemically silver-plated slurry for low-temperature co-fired ceramics, which can meet the requirements of chemical nickel / gold plating process of LTCC substrate and matching of slurry and LTCC green ceramic tape, thereby realizing the full silver chemical plating process of LTCC substrate and avoiding the problem of deformation or warping of the substrate.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention provides a chemically plating silver paste for low temperature co-fired ceramics, which is rolled from 70-90wt% of silver powder, 0.1-7wt% of inorganic glass powder and the balance of an organic carrier;

[0008] Wherein, the inorganic glass powder is composed of B 2 O 3 、SiO 2 、SrO、BaO、ZnO、Al2 O 3 、TiO 2 , K 2 O, MgO, SnO 2 and ZrO 2 composition.

[0009] In a further embodiment, the inorganic glass powder comprises the following components in percentage by mass: 2 O 3 15-30%, SiO 2 15-40%, SrO 10-30%, BaO 10-30%, ZnO 5-15%, Al 2 O 3 1-10%, TiO 2 1-10%, K 2 O is 1-10%, MgO is 1-10%, SnO 2 1-10%, ZrO 2 1-10%.

[0010] In a further embodiment, the silver powder is selected from one or a mixture of two or more of spherical silver powder, flaky silver powder, linear silver powder, and irregular silver powder.

[0011] Preferably, the silver powder is selected from spherical silver powder, and the D50 of the spherical silver powder is 0.5-3.5 μm.

[0012] In a further embodiment, the organic carrier is composed of the following components by mass percentage: 5%-30% organic binder, 5-30% auxiliary agent and the balance organic solvent.

[0013] In a further embodiment, the organic binder is selected from at least one of ethyl cellulose, nitrocellulose, polyvinyl butyral, acrylic resin, and epoxy resin.

[0014] In a further embodiment, the auxiliary agent is selected from at least one of a dispersant, a leveling agent, a plasticizer, a thixotropic agent, and a defoaming agent.

[0015] In a further embodiment, the organic solvent is selected from at least one of diethylene glycol butyl ether, diethylene glycol butyl ether acetate, DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and terpineol.

[0016] The present invention further discloses a method for preparing the above-mentioned chemically plating silver paste, comprising the following steps:

[0017] The silver powder, inorganic glass powder and organic carrier are fully mixed according to the ratio to obtain a slurry;

[0018] The slurry is rolled for multiple times until the slurry fineness reaches the requirement of screen printing, thereby obtaining a silver plating slurry.

[0019] In a further embodiment, the preparation process of the inorganic glass powder is as follows: after uniformly mixing the components in the inorganic glass powder, the mixture is subjected to high-temperature melting, water quenching, ball milling, drying, and sieving through a 300-mesh sieve for later use; and / or, the preparation process of the organic carrier is as follows: after uniformly mixing the components in the organic carrier, the mixture is heated and stirred at 50-100°C until a uniform paste is formed, and then cooled to room temperature for later use.

[0020] The present invention has the following beneficial effects:

[0021] 1) The present invention adopts inorganic glass powder of specific composition. On the one hand, the sintering matching between the glass powder and the green porcelain is controlled to meet the low-temperature co-fired ceramic process conditions; on the other hand, the bonding force between the slurry and the ceramic is increased, and the acid resistance and water resistance of the metallized silver layer are improved to adapt to the chemical nickel / gold plating process.

[0022] 2) The chemically plating silver paste provided in the present invention has good consistency in sintering shrinkage with the LTCC substrate and will not cause warping of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a flow chart of a method for preparing a chemically plating silver paste in a typical embodiment of the present invention;

[0024] Figure 2 This is a diagram showing the effect of printing silver paste in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0027] The first aspect of the present invention discloses a chemically plating silver paste for low temperature co-fired ceramics, which is rolled from 70-90wt% of silver powder, 0.1-7wt% of inorganic glass powder and the balance of an organic carrier;

[0028] Wherein, the inorganic glass powder is composed of B 2 O 3 、SiO 2 、SrO、BaO、ZnO、Al 2 O 3 、TiO2 , K 2 O, MgO, SnO 2 and ZrO 2 composition.

[0029] The inorganic glass powder is B 2 O 3 -SiO 2 -SrO-BaO glass powder, which is based on B 2 O 3 、SiO 2 , SrO, BaO as the main components, and some auxiliary components are added, among which, by introducing Al 2 O 3 with SnO 2 The chemical stability of the inorganic glass powder is increased. On the one hand, the acid resistance and water resistance of the chemically silver-plated slurry are improved. On the other hand, the sintering matching between the slurry and the green porcelain is adjusted, so that the sintering shrinkage rate between the slurry and the green porcelain is consistent, avoiding the problem of warping or deformation of the substrate.

[0030] Preferably, the proportions of the components in the inorganic glass powder are as follows, in terms of mass percentage: 2 O 3 15-30%, SiO 2 15-40%, SrO 10-30%, BaO 10-30%, ZnO 5-15%, Al 2 O 3 1-10%, TiO 2 1-10%, K 2 O is 1-10%, MgO is 1-10%, SnO 2 1-10%, ZrO 2 1-10%.

[0031] The silver powder described herein is not particularly limited, and any type of silver powder conventionally used in the art may be used. Specific examples include, but are not limited to, spherical silver powder, flaky silver powder, linear silver powder, irregular silver powder, or a mixture of two or more thereof.

[0032] Preferably, the silver powder is selected from spherical silver powder, and the D50 of the spherical silver powder is 0.5-3.5 μm, so that the silver particles are closely connected and evenly distributed after sintering to form a dense conductive network, so that the metallization layer has a small square resistance, thereby further improving the performance of the product.

[0033] In a further scheme, the organic carrier described in this article can be composed of conventional organic carriers in the art, which generally include organic adhesives, organic solvents and other additives. The reasonable combination of organic adhesives, organic solvents and additives is conducive to the dispersion of silver powder in the slurry, and the rheology and printability of the slurry are good, meeting the requirements of the metallization layer of the LTCC substrate for printability, which can be adjusted according to the needs of those skilled in the art. In some specific embodiments of the present invention, the organic carrier is composed of 5%-30% organic adhesive, 5-30% additive and the remaining organic solvent in terms of mass percentage. Among them, the organic adhesive can be selected from at least one of ethyl cellulose, nitrocellulose, polyvinyl butyral, acrylic resin, and epoxy resin; the organic solvent can be selected from at least one of diethylene glycol butyl ether, diethylene glycol butyl ether acetate, DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and pinene alcohol; the additive can be selected from at least one of a dispersant, a leveling agent, a plasticizer, a thixotropic agent, and a defoaming agent. It is understandable that the selection of organic binders, organic solvents and additives is not limited to the above examples, and any conventionally used organic binders in the art may be used.

[0034] The second aspect of the present invention provides a method for preparing the chemically silver-plated slurry according to the first aspect of the present invention, such as Figure 1 As shown in FIG. , a method for preparing a chemically plating silver paste in a typical embodiment of the present invention is shown, comprising the following steps:

[0035] Silver powder, inorganic glass powder and organic carrier are fully and uniformly mixed according to the ratio to obtain slurry; the mixing method is not particularly limited, such as high-speed stirring. In some typical embodiments of the present invention, stirring at a speed of 600-2000 rpm for 2-20 minutes is sufficient.

[0036] The slurry is rolled for multiple times until the slurry fineness reaches the requirement of screen printing, thereby obtaining a silver plating slurry. It is understood that the slurry can be rolled using a three-roller mill, and the specific number of times is not particularly limited, as long as the slurry fineness meets the requirement.

[0037] Among them, the preparation of inorganic glass powder and organic carrier can be carried out according to the process well known to those skilled in the art. In some typical embodiments of the present invention, the preparation process of the inorganic glass powder is: after the components in the inorganic glass powder are mixed evenly, they are subjected to high-temperature melting, water quenching, ball milling, drying, and sieve through a 300-mesh screen for use; and / or, the preparation process of the organic carrier is: after the components in the organic carrier are mixed evenly, they are heated and stirred at 50-100°C until a uniform paste is formed, and then cooled to room temperature for use.

[0038] The present invention is described below by means of specific examples. It should be noted that the following specific examples are only for illustrative purposes and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial channels.

[0039] Example 1

[0040] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver plating paste comprises the following components by mass percentage: 72% silver powder, 3% inorganic glass powder, and 25% organic carrier. The silver powder is spherical silver powder with a particle size D50 of 0.5-3.5 μm. The inorganic glass powder comprises the following components by mass percentage: B 2 O 3 20%, SiO 2 20%, SrO 15%, BaO 15%, ZnO 10%, Al 2 O 3 5%, TiO 2 5%, K 2 O is 3%, MgO is 3%, SnO 2 is 2%, ZrO 2 The composition of the organic carrier is calculated by mass, including the following components: 12 parts of ethyl cellulose, 73 parts of pine alcohol, 5 parts of dispersant, 5 parts of plasticizer, and 5 parts of leveling agent.

[0041] The preparation method of the chemically plating silver paste comprises the following specific steps:

[0042] Preparation of inorganic glass powder: Inorganic oxides are weighed in proportion and stirred and mixed, and then melted at high temperature, quenched with water, ball milled, dried, and passed through a 300-mesh sieve for later use;

[0043] Preparation of organic carrier: weigh organic binder, organic solvent and auxiliary agent according to proportion, add them into a double-layer glass reactor, first add organic solvent and auxiliary agent and stir evenly, set heating temperature to 70°C, stirring speed to 240r / min, then slowly add organic binder while stirring until a uniform paste is formed, and cool to room temperature for use;

[0044] Preparation of silver paste: weigh organic carrier, inorganic glass powder and silver powder according to the ratio into a mixing tank, put the mixing tank into a homogenizer, and stir at high speed to make them evenly mixed, wherein the stirring speed is 1000r / min, and the stirring time is 10 minutes; the mixed slurry is rolled into a paste slurry with a three-roll machine until the slurry fineness reaches the requirement of screen printing to obtain the required electronic slurry.

[0045] Example 2

[0046] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver plating paste comprises the following components by mass percentage: 74% silver powder, 1% inorganic glass powder, and 25% organic carrier. The silver powder is spherical silver powder with a particle size D50 of 0.5-3.5 μm; the inorganic glass powder comprises the following components by mass percentage: B 2 O 3 25%, SiO 2 20%, SrO 10%, BaO 20%, ZnO 5%, Al 2 O 3 5%, TiO 2 3%, K 2 O is 3%, MgO is 3%, SnO 2 is 2%, ZrO 2 The composition of the organic carrier is calculated by weight, including the following components: 12 parts of ethyl cellulose, 73 parts of pine alcohol, 5 parts of dispersant, 5 parts of plasticizer, and 5 parts of leveling agent.

[0047] The method for preparing the chemically platable silver paste adopts the same implementation as that of Example 1, except that in the preparation of the silver paste, the stirring speed is 1000 r / min and the stirring time is 15 min.

[0048] Example 3

[0049] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver plating paste comprises the following components by mass percentage: 70% silver powder, 5% inorganic glass powder, and 25% organic carrier. The silver powder is spherical silver powder with a particle size D50 of 0.5-3.5 μm. The inorganic glass powder comprises the following components by mass percentage: B 2 O 3 20%, SiO 2 20%, SrO 10%, BaO 20%, ZnO 10%, Al 2 O 3 3%, TiO 2 5%, K 2 O is 2%, MgO is 3%, SnO 2 is 3%, ZrO 2 The composition of the organic carrier is calculated by weight, including the following components: 12 parts of ethyl cellulose, 73 parts of pine alcohol, 5 parts of dispersant, 5 parts of plasticizer, and 5 parts of leveling agent.

[0050] The method for preparing the chemically platable silver paste adopts the same implementation as that of Example 1, except that in the preparation of the silver paste, the stirring speed is 1000 r / min and the stirring time is 20 min.

[0051] Example 4

[0052] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver plating paste comprises the following components by mass percentage: 77% silver powder, 3% inorganic glass powder, and 20% organic carrier. The silver powder is spherical silver powder with a particle size D50 of 0.5-3.5 μm; the inorganic glass powder comprises the following components by mass percentage: B 2 O 3 20%, SiO 2 20%, SrO 15%, BaO 20%, ZnO 10%, Al 2 O 3 3%, TiO 2 3%, K 2 O is 3%, MgO is 2%, SnO 2 is 2%, ZrO 2 The composition of the organic carrier is calculated by weight, including the following components: 11 parts of ethyl cellulose, 74 parts of pine alcohol, 5 parts of dispersant, 5 parts of plasticizer, and 5 parts of leveling agent.

[0053] The method for preparing the chemically platable silver paste adopts the same implementation as that of Example 1, except that in the preparation of the silver paste, the stirring speed is 1200 r / min and the stirring time is 15 min.

[0054] Example 5

[0055] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver paste comprises the following components by mass percentage: 82% silver powder, 3% inorganic glass powder, and 15% organic carrier. The silver powder is spherical silver powder with a particle size D50 of 0.5-3.5 μm; the inorganic glass powder comprises the following components by mass percentage: B 2 O 3 20%, SiO 2 25%, SrO 10%, BaO 15%, ZnO 10%, Al 2 O 3 5%, TiO 2 5%, K 2 O is 5%, MgO is 2%, SnO 2 is 1%, ZrO 2 The composition of the organic carrier is calculated by weight, including the following components: 10 parts of ethyl cellulose, 75 parts of pine alcohol, 5 parts of dispersant, 5 parts of plasticizer, and 5 parts of leveling agent.

[0056] The method for preparing the chemically platable silver paste adopts the same implementation as that of Example 1, except that in the preparation of the silver paste, the stirring speed is 1200 r / min and the stirring time is 20 min.

[0057] Example 6

[0058] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver paste comprises the following components by mass percentage: 90% silver powder, 0.1% inorganic glass powder, and 9.9% organic carrier. The silver powder is flaky silver powder; the inorganic glass powder comprises the following components by mass percentage: 2 O 3 15%, SiO 2 20%, SrO 25%, BaO 10%, ZnO 5%, Al 2 O 3 1%, TiO 2 3%, K 2 O is 4%, MgO is 2%, SnO 2 is 10%, ZrO 2 The composition of the organic carrier is calculated by mass, including the following components: 5 parts of polyvinyl butyral, 90 parts of diethylene glycol butyl ether, 1 part of dispersant, 1 part of plasticizer, 1 part of leveling agent, 1 part of thixotropic agent, and 1 part of defoaming agent.

[0059] The preparation method of the chemically platable silver-plating paste adopts the same implementation as that of Example 1.

[0060] Example 7

[0061] This embodiment discloses a silver plating paste for low temperature co-fired ceramics. The silver paste comprises the following components by mass percentage: 70% silver powder, 7% inorganic glass powder, and 23% organic carrier. The silver powder is irregular silver powder; the inorganic glass powder comprises the following components by mass percentage: B 2 O 3 30%, SiO 2 15%, SrO 10%, BaO 15%, ZnO 15%, Al 2 O 3 10%, TiO 2 1%, K 2 O is 1%, MgO is 1%, SnO 2 is 1%, ZrO 2 The composition of the organic carrier is calculated by mass, including the following components: 30 parts of epoxy resin, 40 parts of DBE, 6 parts of dispersant, 6 parts of plasticizer, 6 parts of leveling agent, 6 parts of thixotropic agent, and 6 parts of defoaming agent.

[0062] The preparation method of the chemically platable silver-plating paste adopts the same implementation as that of Example 1.

[0063] Comparative Example 1

[0064] This comparative example discloses a silver paste, the composition and preparation process of which are the same as those of Example 1, except that the types of inorganic glass powder used are different. The inorganic glass powder in this comparative example comprises, by mass percentage, 35% CaO, 25% B 2 O 3 33%, SiO 2 is 30%, ZrO 2 is 2%.

[0065] Comparative Example 2

[0066] This comparative example discloses a silver paste, the composition and preparation process of which are the same as those of Example 1, except that the types of inorganic glass powder used are different. The inorganic glass powder in this comparative example, calculated by mass percentage, comprises the following components: Bi 2 O 3 59%, SiO 2 25%, B 2 O 3 10%, Al 2 O 3 is 3%.

[0067] Comparative Example 3

[0068] This comparative example discloses a silver paste, the composition and preparation process of which are basically the same as those of Example 1, except that the composition of the inorganic glass powder used is different. The composition of the inorganic glass powder in this comparative example is: B 2 O 3 20%, SiO 2 20%, SrO 15%, BaO 15%, ZnO 10%, Al 2 O 3 7%, TiO 2 5%, K 2 O is 3%, MgO is 3%, ZrO 2 is 2%.

[0069] Comparative Example 4

[0070] This comparative example discloses a silver paste, the composition and preparation process of which are basically the same as those of Example 1, except that the composition of the inorganic glass powder used is different. The composition of the inorganic glass powder in this comparative example is: 2 O 3 20%, SiO 2 20%, SrO 15%, BaO 15%, ZnO 10%, TiO 2 5%, K2 O is 3%, MgO is 3%, SnO 2 is 7%, ZrO 2 is 2%.

[0071] Performance Test 1-Acid Resistance of Silver Conductor Film

[0072] The silver pastes prepared in Examples 1-7 and Comparative Examples 1-4 were used as experimental samples. The pastes were printed on LTCC green ceramic sheets by screen printing and sintered at 850° C. The sintered substrates were immersed in a 10% mass fraction HCl solution at 25° C. for 30 min. The surface flatness and acid resistance of the silver film layer were tested. The experimental results are shown in Table 1.

[0073] Table 1 Surface smoothness and acid resistance of silver conductor film

[0074] <![CDATA[Surface flatness a > Film shedding Example 1 qualified Not falling off Example 2 qualified Not falling off Example 3 qualified Not falling off Example 4 qualified Not falling off Example 5 qualified Not falling off Example 6 qualified Not falling off Example 7 qualified Not falling off Comparative Example 1 Failure Film shedding Comparative Example 2 Failure Film shedding Comparative Example 3 Failure Not falling off Comparative Example 4 Failure Not falling off

[0075] (Note: a: Surface flatness ≤0.2mm / 50mm is qualified).

[0076] From the test results in Table 1, it can be seen that compared with Examples 1-7 and Comparative Examples 1-4, the B used in the present invention 2 O 3 -SiO 2 -SrO-BaO series inorganic glass powder can improve the acid resistance of the silver film layer, indicating that the addition of the inorganic glass powder is beneficial to improving the bonding strength between the silver conductor film layer and the substrate, and has excellent surface flatness, and will not cause warping and deformation of the substrate.

[0077] Performance Test 2 - Adhesion of Silver Conductor Film on Electroless Nickel / Gold Plated Samples

[0078] The samples in Examples 1-7 and Comparative Examples 1-4 were respectively subjected to silver conductor film layer chemical nickel / gold plating, with the nickel plating thickness being ≥3 μm and the gold plating thickness being ≥0.3 μm. The gold wire bonding performance of the chemically plated samples was evaluated, and a 25 μm gold wire was used to test the gold wire bonding strength. The experimental results are shown in Table 2.

[0079] Table 2 Adhesion results of silver conductor film layer of chemical nickel / gold plated samples

[0080] Appearance Bond strength Example 1 good 9.2g Example 2 good 9.0g Example 3 good 8.8g Example 4 good 9.6g Example 5 good 10.5g Example 6 good 8.7g Example 7 good 9.1g Comparative Example 1 Shedding / Comparative Example 2 Shedding / Comparative Example 3 good 7.6g Comparative Example 4 good 8.3g

[0081] It can be seen from the test results in Table 2 that compared with Examples 1-7 and Comparative Examples 1-4, the B 2 O 3 -SiO 2 -SrO-BaO inorganic glass powder can significantly improve the gold wire bonding strength after silver film layer electroless nickel / gold plating.

[0082] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0083] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A chemically silver-plated slurry for low temperature co-fired ceramics, characterized in that: It is rolled from 70-90wt% of silver powder, 0.1-7wt% of inorganic glass powder and the balance of organic carrier; Among them, the inorganic glass powder is composed of the following components in mass percentage: B2O3 is 15-30%, SiO2 is 15-40%, SrO is 10-30%, BaO is 10-30%, ZnO is 5-15%, Al2O3 is 1-10%, TiO2 is 1-10%, K2O is 1-10%, MgO is 1-10%, SnO2 is 1-10%, and ZrO2 is 1-10%.

2. The chemically platable silver plating paste according to claim 1, characterized in that: The silver powder is selected from one of spherical silver powder, flaky silver powder, linear silver powder, irregular silver powder, or a mixture of two or more thereof.

3. The chemically plating silver paste according to claim 2, characterized in that: The silver powder is selected from spherical silver powder, and the D50 of the spherical silver powder is 0.5-3.5 μm.

4. The chemically platable silver plating paste according to claim 1, characterized in that: The organic carrier is composed of the following components by mass percentage: 5%-30% organic binder, 5%-30% auxiliary agent and the balance organic solvent.

5. The chemically platable silver plating paste according to claim 4, characterized in that: The organic adhesive is selected from at least one of ethyl cellulose, nitrocellulose, polyvinyl butyral, acrylic resin and epoxy resin.

6. The chemically platable silver plating paste according to claim 4, characterized in that: The auxiliary agent is selected from at least one of a dispersant, a leveling agent, a plasticizer, a thixotropic agent, and a defoaming agent.

7. The chemically platable silver plating paste according to claim 4, characterized in that: The organic solvent is selected from at least one of diethylene glycol butyl ether, diethylene glycol butyl ether acetate, DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and terpineol.

8. A method for preparing a chemically plating silver paste as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: The silver powder, inorganic glass powder and organic carrier are fully mixed according to the ratio to obtain a slurry; The slurry is rolled for multiple times until the slurry fineness reaches the requirement of screen printing, thereby obtaining a silver plating slurry.

9. The preparation method according to claim 8, characterized in that: The preparation process of the inorganic glass powder is as follows: after the components in the inorganic glass powder are uniformly mixed, the mixture is subjected to high temperature melting, water quenching, ball milling, drying, and passing through a 300-mesh sieve for later use; And / or, the preparation process of the organic carrier is: after uniformly mixing the components in the organic carrier, heating and stirring at 50-100° C. until a uniform paste is formed, cooling to room temperature for use.

Citation Information

Patent Citations

  • Nickel-gold plateable thick film silver paste, and plating process for low temperature co fired ceramic devices and LTCC devices made therefrom

    CN102149847A

  • Electrode slurry and preparation method

    CN104112490A

  • Low-temperature co-fired microwave dielectric ceramic material and preparation method thereof

    CN107522481A

  • Degradable low-temperature co-fired ceramic and preparation method thereof

    CN108863324A

  • LTCC material with low dielectric constant and preparation method thereof

    CN110436894A