A chelating adsorbent for electroplating wastewater treatment and preparation method thereof

By using raw materials in a specific ratio to form a chelating adsorbent with a multi-network structure, the problem of low copper ion removal efficiency in electroplating wastewater is solved, achieving high-efficiency adsorption and improved stability.

CN115814763BActive Publication Date: 2024-11-08ZHAOQING LINGYU ENVIRONMENTAL PROTECTION IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111454699.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-01
Publication Date
2024-11-08
Estimated Expiration
2041-12-01

AI Technical Summary

Technical Problem

The lack of chelating adsorbents suitable for treating copper ions in various electroplating wastewaters in the current technology results in low copper ion removal efficiency.

Method used

Using a specific ratio of alkylpyridine compounds, alkylbenzene compounds, diluents, carboxymethylated derivatives of cellulose, initiators, and inorganic compounds as raw materials, a chelating adsorbent with a multi-network structure is formed through a cross-linking reaction, thereby enhancing its adsorption capacity for copper ions.

Benefits of technology

It improved the adsorption capacity and selectivity of copper ions in electroplating wastewater, enhanced the stability and generation rate of the adsorbent, and strengthened the adsorption effect on copper ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003387373100000071
    Figure BDA0003387373100000071
Patent Text Reader

Abstract

The present invention relates to the technical field of CO2F9 / 04, and in particular to a chelated adsorbent for electroplating wastewater treatment and a preparation method thereof. A chelated adsorbent for electroplating wastewater treatment, wherein the raw materials for preparing the chelated adsorbent include 20-22% alkylpyridine compounds, 4.5-5.5% alkylbenzene compounds, 16-20% diluents, 0.5-1% carboxymethylated derivatives of cellulose, 2.2-2.8% initiators, 4-6% inorganic compounds, and the remainder of water, by weight percentage. The chelated adsorbent for electroplating wastewater treatment prepared by the present invention has a multi-network structure, can efficiently form a multi-coordinated complex with metal ions, and adsorb metal ions in electroplating wastewater, in particular, adsorb copper ions in electroplating wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of CO2F9 / 04, and in particular to a chelating adsorbent for electroplating wastewater treatment and a preparation method thereof. Background Art

[0002] A Chinese patent with patent application number CN202011402845.5 discloses a process for treating and reusing electroplating copper-containing wastewater and its application. Chelating resin is used in the chelating adsorption section of the process for treating and reusing electroplating copper-containing wastewater. It is mainly used to treat electroplating copper-containing wastewater containing sulfonic acid pollutants. There is no disclosure on the removal of copper from wastewater in various electroplating processes. Therefore, it is necessary to provide a chelating adsorbent that can be used to treat various wastewaters to remove copper, which is the main technical problem that needs to be solved at present. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a chelated adsorbent for electroplating wastewater treatment. The raw materials for preparation include 20-22% alkylpyridine compounds, 4.5-5.5% alkylbenzene compounds, 16-20% diluents, 0.5-1% carboxymethylated derivatives of cellulose, 2.2-2.8% initiators, 4-6% inorganic compounds, and the balance water, calculated by mass percentage.

[0004] Preferably, the alkylpyridine compound is selected from one or more of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, and 2-methyl-5-vinylpyridine.

[0005] Preferably, the alkyl pyridine compound is a mixture of 4-vinyl pyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinyl pyridine, and the weight ratio of 4-vinyl pyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinyl pyridine is 1:(1-4):(0.5-3).

[0006] Preferably, the weight ratio of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinylpyridine is 1:(2-3):(1-2).

[0007] Preferably, the alkylbenzene compound includes a benzene compound containing an unsaturated bond.

[0008] Preferably, the alkylbenzene compound is p-divinylbenzene.

[0009] The applicant unexpectedly discovered in the experiment that when a mixture consisting of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinylpyridine is selected as the preparation raw material, especially when the weight ratio of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinylpyridine is 1:(1-4):(0.5-3), and especially when the weight ratio of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer and 2-methyl-5-vinylpyridine is 1:(2-3):(1-2), the chelating adsorbent for electroplating wastewater treatment obtained by cross-linking reaction under the action of divinylbenzene can form a multi-network structure, and can efficiently form a multi-coordinated complex with metal ions when used, thereby being able to adsorb metal ions contained in the electroplating wastewater, especially copper ions in the electroplating wastewater. The possible reason is that the chelating adsorbent can form a multi-network structure and has a certain selectivity for copper ions, thereby increasing the adsorption amount of copper ions in the electroplating wastewater.

[0010] Preferably, the diluent comprises xylene and diethyl tartrate.

[0011] Preferably, the weight ratio of xylene to diethyl tartrate is (1.5-3):1.

[0012] Preferably, the weight ratio of xylene to diethyl tartrate is (1.8-2.5):1.

[0013] Preferably, the weight ratio of xylene to diethyl tartrate is 2:1.

[0014] The applicant unexpectedly discovered in the experiment that when xylene and diethyl tartrate are used as diluents, when the weight ratio of xylene to diethyl tartrate is (1.5-3):1, the chelate adsorbent has a certain storage stability, especially when the weight ratio of xylene to diethyl tartrate is (1.8-2.5):1, especially when the weight ratio of xylene to diethyl tartrate is 2:1, the prepared chelate adsorbent for electroplating wastewater treatment has good storage stability, and the absorption of metal ions by the chelate adsorbent will not be affected by long storage time. Attachment, especially the adsorption of copper ions, can efficiently form multi-coordination complexes with metal ions, adsorb metal ions in electroplating wastewater, especially copper ions in electroplating wastewater. The possible reason is that under the action of xylene and diethyl tartrate, the multi-network structure of the chelating adsorbent has an enhanced expansion ability in electroplating wastewater, which increases the contact area between the molecular chain of the chelating adsorbent and the heavy metal ions in the electroplating wastewater, has a certain selectivity for copper ions, and improves the adsorption capacity of metal ions, especially the adsorption amount of copper ions.

[0015] Preferably, the carboxymethylated derivative of cellulose is selected from sodium carboxymethylcellulose or hydroxypropyl methylcellulose.

[0016] Preferably, the carboxymethylated derivative of cellulose is sodium carboxymethyl cellulose.

[0017] Preferably, the initiator is azobisisobutyronitrile.

[0018] Preferably, the inorganic compound is ammonium sulfite.

[0019] Preferably, the water is deionized water.

[0020] The applicant unexpectedly discovered in the experiment that mixing ammonium sulfite, sodium carboxymethyl cellulose and water and adding them to a mixture consisting of 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, diethyl tartrate and azobisisobutyronitrile has a synergistic effect, which can increase the generation rate of the chelated adsorbent for electroplating wastewater treatment and improve the stability of the chelated adsorbent.

[0021] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0022] S1, adding an alkyl pyridine compound, an alkyl benzene compound, a diluent, and an initiator into a stirring device and mixing and stirring to obtain a mixture a;

[0023] S2, adding the carboxymethylated derivative of cellulose, the inorganic compound and water into a stirring device and mixing and stirring to obtain a mixture b;

[0024] S3, adding mixture a and mixture b into a reaction kettle, stirring for 15-30 min under a nitrogen atmosphere, heating to 60-70 degrees Celsius and stirring for 1-3 hours, and then heating to 80-85 degrees Celsius and stirring for 6-10 hours to polymerize to obtain a polymer and cool;

[0025] S4. Use deionized water at 80-85 degrees Celsius to wash and filter the polymer, then add it to a Soxhlet extractor and use ethanol to extract for 3-7 hours and then dry it to obtain a chelating adsorbent for electroplating wastewater treatment.

[0026] Beneficial Effects

[0027] The chelated adsorbent for electroplating wastewater treatment prepared by the present invention has high adsorption capacity for copper ions in water and high treatment efficiency for copper-containing electroplating wastewater.

[0028] The chelated adsorbent for electroplating wastewater treatment prepared by the present invention has a multi-network structure, can efficiently form a multi-coordination complex with metal ions, adsorb metal ions in electroplating wastewater, has a certain selectivity for copper ions, and has good adsorption for copper ions in electroplating wastewater.

[0029] The present invention selects xylene and diethyl tartrate as diluents. Under the action of xylene and diethyl tartrate, the multi-network structure of the chelated adsorbent for electroplating wastewater treatment has enhanced expansion ability in electroplating wastewater, increases the contact area between the molecular chain of the chelated adsorbent and the heavy metal ions in the electroplating wastewater, improves the adsorption capacity of metal ions, has a certain selectivity for copper ions, and improves the adsorption amount of copper ions.

[0030] The invention improves the generation rate of a chelate adsorbent for electroplating wastewater treatment by mixing ammonium sulfite, sodium carboxymethyl cellulose and water, thereby improving the stability of the chelate adsorbent. DETAILED DESCRIPTION

[0031] Example 1

[0032] A chelating adsorbent for electroplating wastewater treatment. The raw materials for preparation include, by weight percentage, 3.5% of 4-vinylpyridine, 10.5% of 2-vinyl-6-methyl-pyridine homopolymer, 7% of 2-methyl-5-vinylpyridine, 5% of divinylbenzene, 12% of xylene, 6% of diethyl tartrate, 0.7% of sodium carboxymethyl cellulose, 2.5% of azobisisobutyronitrile, 5% of ammonium sulfite and 47.8% of deionized water.

[0033] The CAS number of the 4-vinylpyridine is 100-43-6.

[0034] The CAS number of the 2-vinyl-6-methyl-pyridine homopolymer is 27680-96-2.

[0035] The CAS number of the 2-methyl-5-vinylpyridine is 140-76-1.

[0036] The CAS number of the sodium carboxymethyl cellulose is 9004-32-4.

[0037] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0038] S1, adding 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, diethyl tartrate and azobisisobutyronitrile into a stirring device and mixing and stirring to obtain a mixture a;

[0039] S2, adding sodium carboxymethyl cellulose, ammonium sulfite and deionized water into a stirring device and mixing and stirring to obtain a mixture b;

[0040] S3, adding mixture a and mixture b into a reactor, stirring for 15 min under a nitrogen atmosphere, heating to 65 degrees Celsius and stirring for 1.5 hours, and then heating to 85 degrees Celsius and stirring for 8 hours to polymerize to obtain a polymer and cool;

[0041] S4. The polymer is washed and filtered with deionized water at 85 degrees Celsius, and then added to a Soxhlet extractor and extracted with ethanol for 5 hours and then dried to obtain a chelating adsorbent for electroplating wastewater treatment.

[0042] Example 2

[0043] A chelating adsorbent for electroplating wastewater treatment. The raw materials for preparation include, by weight percentage, 4% of 4-vinylpyridine, 10% of 2-vinyl-6-methyl-pyridine homopolymer, 6% of 2-methyl-5-vinylpyridine, 4.5% of divinylbenzene, 12% of xylene, 6% of diethyl tartrate, 0.6% of sodium carboxymethyl cellulose, 2.2% of azobisisobutyronitrile, 5% of ammonium sulfite and 49.8% of deionized water.

[0044] The CAS number of the 4-vinylpyridine is 100-43-6.

[0045] The CAS number of the 2-vinyl-6-methyl-pyridine homopolymer is 27680-96-2.

[0046] The CAS number of the 2-methyl-5-vinylpyridine is 140-76-1.

[0047] The CAS number of the sodium carboxymethyl cellulose is 9004-32-4.

[0048] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0049] S1, adding 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, diethyl tartrate and azobisisobutyronitrile into a stirring device and mixing and stirring to obtain a mixture a;

[0050] S2, adding sodium carboxymethyl cellulose, ammonium sulfite and deionized water into a stirring device and mixing and stirring to obtain a mixture b;

[0051] S3, adding mixture a and mixture b into a reactor, stirring for 15 min under a nitrogen atmosphere, heating to 65 degrees Celsius and stirring for 1.5 hours, and then heating to 85 degrees Celsius and stirring for 8 hours to polymerize to obtain a polymer and cool;

[0052] S4. The polymer is washed and filtered with deionized water at 85 degrees Celsius, and then added to a Soxhlet extractor and extracted with ethanol for 5 hours and then dried to obtain a chelating adsorbent for electroplating wastewater treatment.

[0053] Example 3

[0054] A chelating adsorbent for electroplating wastewater treatment. The raw materials for preparation include, by weight percentage, 5.5% of 4-vinylpyridine, 11% of 2-vinyl-6-methyl-pyridine homopolymer, 5.5% of 2-methyl-5-vinylpyridine, 5.5% of divinylbenzene, 12% of xylene, 6% of diethyl tartrate, 1% of sodium carboxymethyl cellulose, 2.8% of azobisisobutyronitrile, 5% of ammonium sulfite and 45.7% of deionized water.

[0055] The CAS number of the 4-vinylpyridine is 100-43-6.

[0056] The CAS number of the 2-vinyl-6-methyl-pyridine homopolymer is 27680-96-2.

[0057] The CAS number of the 2-methyl-5-vinylpyridine is 140-76-1.

[0058] The CAS number of the sodium carboxymethyl cellulose is 9004-32-4.

[0059] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0060] S1, adding 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, diethyl tartrate and azobisisobutyronitrile into a stirring device and mixing and stirring to obtain a mixture a;

[0061] S2, adding sodium carboxymethyl cellulose, ammonium sulfite and deionized water into a stirring device and mixing and stirring to obtain a mixture b;

[0062] S3, adding mixture a and mixture b into a reactor, stirring for 15 min under a nitrogen atmosphere, heating to 65 degrees Celsius and stirring for 1.5 hours, and then heating to 85 degrees Celsius and stirring for 8 hours to polymerize to obtain a polymer and cool;

[0063] S4. The polymer is washed and filtered with deionized water at 85 degrees Celsius, and then added to a Soxhlet extractor and extracted with ethanol for 5 hours and then dried to obtain a chelating adsorbent for electroplating wastewater treatment.

[0064] Example 4

[0065] A chelating adsorbent for electroplating wastewater treatment, wherein the raw materials for preparation include, by weight percentage, 7% 4-vinylpyridine, 14% 2-methyl-5-vinylpyridine, 5% divinylbenzene, 12% xylene, 6% diethyl tartrate, 0.7% sodium carboxymethyl cellulose, 2.5% azobisisobutyronitrile, 5% ammonium sulfite and 47.8% deionized water.

[0066] The CAS number of the 4-vinylpyridine is 100-43-6.

[0067] The CAS number of the 2-vinyl-6-methyl-pyridine homopolymer is 27680-96-2.

[0068] The CAS number of the 2-methyl-5-vinylpyridine is 140-76-1.

[0069] The CAS number of the sodium carboxymethyl cellulose is 9004-32-4.

[0070] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0071] S1, adding 4-vinylpyridine, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, diethyl tartrate and azobisisobutyronitrile into a stirring device and mixing and stirring to obtain a mixture a;

[0072] S2, adding sodium carboxymethyl cellulose, ammonium sulfite and deionized water into a stirring device and mixing and stirring to obtain a mixture b;

[0073] S3, adding mixture a and mixture b into a reactor, stirring for 15 min under a nitrogen atmosphere, heating to 65 degrees Celsius and stirring for 1.5 hours, and then heating to 85 degrees Celsius and stirring for 8 hours to polymerize to obtain a polymer and cool;

[0074] S4. The polymer is washed and filtered with deionized water at 85 degrees Celsius, and then added to a Soxhlet extractor and extracted with ethanol for 5 hours and then dried to obtain a chelating adsorbent for electroplating wastewater treatment.

[0075] Example 5

[0076] A chelating adsorbent for electroplating wastewater treatment. The raw materials for preparation include, by mass percentage, 3.5% of 4-vinylpyridine, 10.5% of 2-vinyl-6-methyl-pyridine homopolymer, 7% of 2-methyl-5-vinylpyridine, 5% of divinylbenzene, 18% of xylene, 0.7% of sodium carboxymethyl cellulose, 2.5% of azobisisobutyronitrile, 5% of ammonium sulfite and 47.8% of deionized water.

[0077] The CAS number of the 4-vinylpyridine is 100-43-6.

[0078] The CAS number of the 2-vinyl-6-methyl-pyridine homopolymer is 27680-96-2.

[0079] The CAS number of the 2-methyl-5-vinylpyridine is 140-76-1.

[0080] The CAS number of the sodium carboxymethyl cellulose is 9004-32-4.

[0081] A method for preparing a chelating adsorbent for electroplating wastewater treatment comprises the following steps:

[0082] S1, adding 4-vinylpyridine, 2-vinyl-6-methyl-pyridine homopolymer, 2-methyl-5-vinylpyridine, divinylbenzene, xylene, and azobisisobutyronitrile into a stirring device and mixing and stirring to obtain a mixture a;

[0083] S2, adding sodium carboxymethyl cellulose, ammonium sulfite and deionized water into a stirring device and mixing and stirring to obtain a mixture b;

[0084] S3, adding mixture a and mixture b into a reactor, stirring for 15 min under a nitrogen atmosphere, heating to 65 degrees Celsius and stirring for 1.5 hours, and then heating to 85 degrees Celsius and stirring for 8 hours to polymerize to obtain a polymer and cool;

[0085] S4. The polymer is washed and filtered with deionized water at 85 degrees Celsius, and then added to a Soxhlet extractor and extracted with ethanol for 5 hours and then dried to obtain a chelating adsorbent for electroplating wastewater treatment.

[0086] Performance Testing

[0087] 1. Copper ion adsorption

[0088] Test method:

[0089] (1) Prepare standard solution

[0090] The absorbance of CuSO4.5H2O standard solution with different concentrations was measured by UV spectrophotometer, and the starting Cu 2+ concentration.

[0091] (2) Prepare the sample

[0092] The chelate adsorbents for electroplating wastewater treatment prepared in Examples 1-5 were placed for 0 days and 180 days, respectively, and then placed on a shaker for 3 hours (25°C, 150 r / min). The absorbance of the supernatant was measured and the Cu content in the supernatant was calculated. 2+ concentration, calculate the effect of resin on Cu 2+The adsorption capacity of the samples was 0.147 W / m and the test results are shown in Table 1.

[0093] Table 1

[0094]

Claims

1. A chelating adsorbent for electroplating wastewater treatment, characterized in that: The raw materials include 20-22% alkylpyridine compounds, 4.5-5.5% alkylbenzene compounds, 16-20% diluents, 0.5-1% carboxymethylated derivatives of cellulose, 2.2-2.8% initiators, 4-6% inorganic compounds, and the balance water, in terms of mass percentage. The alkyl pyridine compound is a mixture of 4-vinyl pyridine, 2-vinyl-6-methyl-pyridine homopolymer, and 2-methyl-5-vinyl pyridine, wherein the weight ratio of 4-vinyl pyridine, 2-vinyl-6-methyl-pyridine homopolymer, and 2-methyl-5-vinyl pyridine is 1:(1-4):(0.5-3); The diluent includes xylene and diethyl tartrate; The weight ratio of xylene to diethyl tartrate is (1.5-3):1; The alkylbenzene compound is p-divinylbenzene; The inorganic compound is ammonium sulfite.

2. The chelate adsorbent for electroplating wastewater treatment according to claim 1, characterized in that: The weight ratio of the 4-vinyl pyridine, the 2-vinyl-6-methyl-pyridine homopolymer and the 2-methyl-5-vinyl pyridine is 1:(2-3):(1-2).

3. The chelating adsorbent for electroplating wastewater treatment according to claim 1, characterized in that: The weight ratio of xylene to diethyl tartrate is (1.8-2.5):

1.

4. The chelating adsorbent for electroplating wastewater treatment according to claim 1, characterized in that: The carboxymethylated derivative of cellulose is selected from sodium carboxymethyl cellulose or hydroxypropyl methyl cellulose.

5. The method for preparing a chelating adsorbent for electroplating wastewater treatment according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, adding an alkyl pyridine compound, an alkyl benzene compound, a diluent, and an initiator into a stirring device and mixing and stirring to obtain a mixture a; S2, adding the carboxymethylated derivative of cellulose, the inorganic compound and water into a stirring device and mixing and stirring to obtain a mixture b; S3, adding mixture a and mixture b into a reaction kettle, stirring for 15-30 min under a nitrogen atmosphere, heating to 60-70 degrees Celsius and stirring for 1-3 hours, and then heating to 80-85 degrees Celsius and stirring for 6-10 hours to polymerize to obtain a polymer and cool; S4. Use deionized water at 80-85 degrees Celsius to wash and filter the polymer, then add it to a Soxhlet extractor and use ethanol to extract for 3-7 hours and then dry it to obtain a chelating adsorbent for electroplating wastewater treatment.