Nickel- and titanium-doped RP structure oxides and their reduced products, preparation and application

By using RP structure oxides doped with nickel and titanium as anode material in solid oxide electrolytic cells, the problems of insufficient catalytic activity and easy carbon deposition in existing anode materials are solved, efficient ethylene production is achieved, and the battery is improved Performance and ethylene selectivity and reduce costs.

CN115818730BActive Publication Date: 2024-11-19BEI JING HUI JU XIN NENG YUAN KE JI YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211034355.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-08-27
Filing Date
2022-08-26
Publication Date
2024-11-19
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

The existing solid oxide electrolytic cell anode materials have problems such as insufficient catalytic activity, easy carbon deposition and sulfur poisoning in the catalytic ethylene production process, resulting in attenuation of battery performance and low ethylene selectivity.

Method used

Using an oxide with a Ruddlesden-Popper (RP) structure doped with nickel and titanium as an anode material, Sr3Fe1.5-xNixTi0 is formed by doping nickel (Ni) and titanium (Ti) in strontium ferrite (Sr3Fe2O7)-based material. .5O7-δ structure and hydrogen reduction treatment forms an oxide loaded with nickel nanoparticles as the anode of the solid oxide electrolytic cell.

Benefits of technology

It improves the electrocatalytic performance and stability of ethane, enhances the resistance to carbon deposits, improves the selectivity and conversion of ethylene, and is low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115818730B_ABST
    Figure CN115818730B_ABST
Patent Text Reader

Abstract

The present invention relates to an RP structure oxide doped with nickel and titanium and its reduced product, preparation and application, belonging to the technical field of solid oxide electrolytic cells. The oxide is Sr3Fe 1.5‑ x Ni x Ti 0.5 O 7‑δ , 0<X≤0.15, δ represents the number of randomly generated oxygen vacancies; the oxide is placed in a reducing atmosphere for reduction treatment to obtain its reduced product, which is an oxide Ni@Sr3Fe with a RP structure doped with nickel and titanium and loaded with nickel nanoparticles. 1.5‑ x Ni x Ti 0.5 O 7‑δ .Ni@Sr3Fe 1.5‑x Ni x Ti 0.5 O 7‑δ The invention has nickel metal particles with high catalytic activity and good electronic conductive phase, and is suitable for being used as anode of solid oxide electrolytic cells, especially as anode of solid oxide electrolytic cells for ethane dehydrogenation to ethylene; it has excellent catalytic performance, good stability and good anti-coking performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an oxide doped with nickel and titanium and having an RP structure, and a reduced product thereof, and preparation and application thereof, belonging to the technical field of solid oxide electrolytic cells. Background Art

[0002] Ethylene is a basic raw material for the chemical industry. Currently, most ethylene is produced by steam cracking of naphtha in industry. Due to the high energy consumption and serious carbon deposition during the cracking process, research and development of new ethylene production technology is of great significance.

[0003] Compared with the traditional ethane steam cracking process, the ethane direct oxidative dehydrogenation (O2-ODH) process is expected to save more than 30% energy due to its exothermic reaction and lower operating temperature. However, the application of this technology also faces many challenges, such as the easy formation of COx and coke, high safety risks, and the need for a large amount of inert gas dilution to keep the reaction mixture away from the flammable zone, which greatly increases equipment investment and operating costs.

[0004] Ethane oxidative dehydrogenation to ethylene can be achieved through a solid oxide electrolyzer (SOEC), which is a device that can convert electrical energy from renewable clean energy into chemical energy. It has the characteristics of high energy conversion efficiency, high efficiency and flexibility. In recent years, SOEC has attracted attention again due to environmental and energy issues.

[0005] SOEC can solve the safety issues caused by excess oxygen in direct oxidation, and will not form by-products such as coke, which can reduce energy consumption; it can kinetically reduce the internal resistance of the battery, thereby improving the electrolysis efficiency.

[0006] The SOEC electrolytic cell consists of two porous electrodes and a dense electrolyte. Under the action of an external electric field, CO2 obtains electrons at the cathode and is converted into CO and oxygen ions (O 2- ), oxygen ions are transferred to the anode through the electrolyte, combined with hydrogen ions to form water, and lose electrons. The hydrogen ions from the ethane dissociation products are continuously consumed, promoting the further conversion of ethane. The oxygen ions are also continuously consumed, which significantly improves the conversion rate of carbon dioxide. The introduction of ethane at the anode reduces the open circuit voltage required by the electrolytic cell and reduces the electrical energy required for the electrolysis reaction.

[0007] Ethane dehydrogenation occurs at the anode of the electrolytic cell. Suitable anode materials are the guarantee for improving ethane conversion and ethylene selectivity. Traditional anode materials Ni / YSZ will have serious carbon deposition and sulfur poisoning when catalyzing hydrocarbon fuels. Long-term operation will also cause Ni sintering and loss of catalytic activity, resulting in battery performance degradation. In order to achieve stable operation of hydrocarbon fuel catalytic oxidation, it is necessary to explore new anode alternative materials. In addition to traditional Ni / YSZ metal ceramic electrodes, mixed ion conductors (MIECs) have attracted much attention from researchers due to their excellent mixed ion electronic conductivity, good electrocatalytic activity, excellent redox stability, resistance to carbon deposition, and resistance to sulfur poisoning. At present, there are three main types of MIECs used for SOEC anodes: 1. Perovskite oxides; 2. Double-layer perovskite oxides; 3. Ruddlesden-Popper (RP) oxides, etc. However, the electrocatalytic activity of such materials is significantly lower than that of traditional Ni-YSZ metal ceramic electrodes.

[0008] In the prior art, there is little research on RP oxides that have application value as new solid oxide electrolytic cell anode materials. RP oxides are commonly used SOFC cathode materials due to their good oxygen ion conductivity, but are currently rarely used as solid oxide electrolytic cell anode materials. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (LSCF) Due to the adsorption of a large number of oxygen species on the surface of the material, ethane will be deeply oxidized, and the ethylene selectivity in the ethane product is low. There is a document that Wang et al. modified and impregnated Al2O3 on the surface of LSCF to optimize the surface structure composition, thereby improving the ethane selectivity. Summary of the invention

[0009] In view of the problems existing in the anode materials of solid oxide electrolysis cells, the purpose of the present invention is to provide an oxide of RP structure doped with nickel and titanium and its reduced product, preparation and application. The oxide has both a highly catalytically active metal structure and a stable RP oxide structure. The reduced product obtained after hydrogen reduction treatment, i.e., an oxide of RP structure loaded with nickel nanoparticles, can be used as an anode of a solid oxide electrolysis cell and has the characteristics of excellent ethane electrocatalytic performance, good stability, low cost, etc.

[0010] To achieve the purpose of the present invention, the following technical solutions are provided.

[0011] An RP structured oxide doped with nickel and titanium, wherein the oxide is formed by doping nickel (Ni) and titanium (Ti) in a strontium ferrite (Sr3Fe2O7) based material, and the composition expression thereof is Sr3Fe 1.5-x Ni xTi 0.5 O 7-δ , where 0<X≤0.15 and δ represents the number of randomly generated oxygen vacancies.

[0012] A method for preparing the RP structured oxide doped with nickel and titanium according to the present invention, the preparation method comprises the following steps:

[0013] (1) According to Sr3Fe 1.5-x Ni x Ti 0.5 O 7-δ The contents of strontium (Sr), iron (Fe), nickel (Ni) and titanium (Ni) in the composition expression are as follows: weigh a strontium source, an iron source, a nickel source and a titanium source, and place them in a solvent to fully dissolve them to obtain a mixed solution;

[0014] Wherein, the strontium source is strontium acetate, strontium nitrate or strontium carbonate; preferably strontium nitrate or strontium acetate.

[0015] The iron source was ferric nitrate.

[0016] The nickel source was nickel nitrate.

[0017] The titanium source is tetrabutyl titanate.

[0018] The solvent was N,N-dimethylformamide (DMF).

[0019] (2) adding the acid to the mixed solution obtained in step (1), and stirring at 80° C. until a transparent yellow gel is formed;

[0020] Wherein, the acid is citric acid, or citric acid and glycine.

[0021] When the acid is citric acid, the ratio of the citric acid to the total molar number of metal cations in the mixed solution is 1 to 2:1, preferably 1:1.

[0022] When the acid is citric acid and glycine, the ratio of the total molar number of citric acid, glycine and the metal cations in the mixed solution is 1-2:1-2:1, preferably 1:1:1.

[0023] (3) heating the gel obtained in step (2) to 250° C. to 300° C. to obtain a powder;

[0024] (4) calcining the powder obtained in step (3) at 800° C. to 1200° C. for 6 h to 10 h to obtain an oxide of RP structure doped with nickel and titanium.

[0025] A reduced product of the RP structured oxide doped with nickel and titanium according to the present invention, i.e., an RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles, has a composition expression of Ni@Sr3Fe 1.5-x Nix Ti 0.5 O 7-δ , where 0<X≤0.15 and δ represents the number of randomly generated oxygen vacancies.

[0026] A method for preparing a reduced product of an oxide of RP structure doped with nickel and titanium according to the present invention, the preparation method comprises the following steps:

[0027] The RP structured oxide doped with nickel and titanium described in the present invention is placed in a reducing atmosphere and subjected to reduction treatment at 600° C. to 900° C. for 1 h to 20 h to obtain a reduced product of the RP structured oxide doped with nickel and titanium, i.e., an RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles.

[0028] Wherein, the reducing atmosphere is a mixture of hydrogen and argon, in which the volume fraction of hydrogen accounts for 5% to 20% of the volume fraction of the mixed gas.

[0029] An application of the nickel- and titanium-doped RP structured oxide loaded with nickel nanoparticles according to the present invention is used as an anode of a solid oxide electrolytic cell, in particular as an anode of a solid oxide electrolytic cell for dehydrogenating ethane to produce ethylene; the application steps are as follows:

[0030] A mixed solution is added to an oxide of RP structure doped with nickel and titanium described in the present invention to prepare an electrode slurry, the electrode slurry is evenly scraped on an electrolyte, calcined at 1000° C. to 1200° C. for 2 h to 5 h, then placed in a mixture of hydrogen and argon, and in-situ reduced at 800° C. for 5 h to obtain an anode on the electrolyte, wherein the material of the anode is a porous oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles.

[0031] The mixed solution is prepared by mixing ethyl cellulose, soluble starch and pinene alcohol.

[0032] The electrolyte is an electrolyte commonly used in the field of solid oxide electrolysis cells.

[0033] Preferably, the electrolyte is yttria-stabilized zirconia coated with a transition layer, wherein the transition layer is gadolinium-doped cerium oxide, and preferably, the molar fraction of yttria in the yttria-stabilized zirconia is 8% (abbreviated as 8-YSZ).

[0034] In the mixed gas, the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0035] Beneficial Effects

[0036] 1. The present invention provides an oxide of RP structure doped with nickel and titanium, wherein the oxide has both a highly catalytically active metal structure and a stable RP oxide structure.

[0037] 2. The present invention provides an oxide of RP structure doped with nickel and titanium, wherein the reduced product obtained after hydrogen reduction treatment is an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles, having nickel metal particles with high catalytic activity and a good electronic conductive phase.

[0038] 3. The present invention provides a method for preparing an oxide of RP structure doped with nickel and titanium, wherein citric acid and glycine are used as complexing agents to complex metal ions together; the gel is heated to 250°C to 300°C to remove organic matter in the gel; the obtained powder is calcined at 1100°C to 1200°C for 6h to 10h to remove nitrogen oxides in the powder and to rearrange atoms by high temperature; the oxide is placed in a reducing atmosphere and reduced at 600°C to 900°C for 1h to 20h, because the metal oxide absorbs oxygen in the reducing atmosphere and is reduced, and the metal ions are reduced to low-valent or even precipitated elements, thereby constructing a metal-oxide interface.

[0039] 4. The present invention provides a reduced product of an oxide of RP structure doped with nickel and titanium, wherein the reduced product is an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles, has nickel metal particles with high catalytic activity and a good electronic conductive phase, and is suitable for use as an anode of a solid oxide electrolytic cell, in particular as an anode of a solid oxide electrolytic cell for dehydrogenating ethane to produce ethylene; compared with other anode materials, the reduced product has excellent catalytic performance, good stability and anti-carbon deposition performance, and is superior to some solid oxide electrolytic cell anode materials in the prior art.

[0040] 5. The present invention provides a method for preparing a reduced product of an oxide of RP structure doped with nickel and titanium, wherein the reduced product is obtained by subjecting an oxide of RP structure doped with nickel and titanium described in the present invention to hydrogen reduction treatment.

[0041] 6. The present invention provides an application of a reduced product of an oxide of RP structure doped with nickel and titanium. Since the reduced material will be reoxidized in a high-temperature oxidizing atmosphere, the oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles cannot be used directly when used as an anode of a solid oxide electrolytic cell. Instead, it must be made into an electrode slurry through its precursor, an oxide of RP structure doped with nickel and titanium, and the electrode slurry is coated on an electrolyte for reduction treatment to obtain the reduced product. The nickel metal nanoparticles are in situ grown and anchored on the surface of the anode substrate, indicating that there is a strong interaction at the metal-oxide interface, which not only prevents the sintering of the metal particles, but also improves the surface structure composition, optimizes the connection between the interface composition and the electrocatalytic performance of ethane, has good structural stability, increases catalytic active sites, improves conversion rate and selectivity, enhances anti-carbon deposition performance, and has the advantage of low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1a The X-ray diffraction (XRD) spectra of the three RP structure oxides doped with nickel and titanium prepared in Example 1 are as follows:

[0043] Figure 1b 1 is the X-ray diffraction (XRD) spectrum of the reduced products of the three RP structured oxides doped with nickel and titanium prepared in Example 1.

[0044] Figure 2 It is Ni@Sr3Fe in Example 1 1.4 Ni 0.1 Ti 0.5 O 7-δ Scanning electron microscope (SEM) image.

[0045] Figure 3 The performance of the three anode materials in Example 1 as anodes of solid oxide electrolysis cells for electrolysis of ethane to ethylene. DETAILED DESCRIPTION

[0046] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0047] Example 1

[0048] A RP structured oxide (Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ), the preparation method comprising the following steps:

[0049] (1) According to Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ The contents of strontium, iron, nickel and titanium in the composition expression were calculated by weighing 6.3489 g (0.03 mol) of strontium nitrate, 5.656 g (0.014 mol) of iron nitrate, 0.29079 g (0.001 mol) of nickel nitrate and 1.6995 g (0.005 mol) of tetrabutyl titanate, and dissolving them fully in 400 ml of solvent N,N-dimethylformamide (DMF) to obtain a mixed solution.

[0050] (2) adding 10.507 g of citric acid to the mixed solution obtained in step (1), and stirring at 80° C. until a transparent yellow gel is formed;

[0051] The ratio of the total molar number of citric acid to the total molar number of metal cations in the mixed solution is 1:1.

[0052] (3) The gel prepared in step (2) is heated to 250° C. and subjected to spontaneous combustion to obtain a powder.

[0053] (4) The powder obtained in step (3) is calcined at 1200° C. for 6 h to obtain an oxide of RP structure doped with nickel and titanium.

[0054] (5) placing the RP structured oxide doped with nickel and titanium obtained in step (4) in a reducing atmosphere and treating it at 800° C. for 5 h to obtain a reduced product of the RP structured oxide doped with nickel and titanium, i.e., an RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles.

[0055] The reducing atmosphere is a mixture of hydrogen and argon, in which the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0056] A RP structured oxide (Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ) in the preparation method of Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ Replaced by Sr3Fe 1.35 Ni 0.15 Ti 0.5 O 7-δ and Sr3Fe 1.45 Ni 0.05 Ti 0.5 O 7-δ The remaining steps are the same as those in Example 1, and two other RP structure oxides doped with nickel and titanium and their reduced products are prepared respectively.

[0057] The following tests and observations were conducted on the three RP structure oxides doped with nickel and titanium and their reduced products obtained in this embodiment:

[0058] (1) X-ray diffraction (XRD) test

[0059] The XRD test instrument used was the X'Pert PRO MPD produced by PANalytical, with a current of 40 mA, a voltage of 40 kV, a Cu target Kα ray, a scanning range of 20° to 80°, and a scanning speed of 10° min -1 .

[0060] The test results are shown in Figure 1. Figure 1a The XRD spectra of three RP structure oxides doped with nickel and titanium show that their structural compositions are Sr3Fe 1.35 Ni0.15 Ti 0.5 O 7-δ 、Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ and Sr3Fe 1.45 Ni 0.05 Ti 0.5 O 7-δ . Figure 1b The XRD spectra of three RP structure oxides doped with nickel and titanium, that is, three RP structure oxides doped with nickel and titanium loaded with nickel nanoparticles, have no change in the main phase structure, indicating that the material structure has excellent reduction stability. Combined with the SEM observation results, it is proved that the structural composition is Ni@Sr3Fe 1.35 Ni 0.15 Ti 0.5 O 7-δ 、Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ and Ni@Sr3Fe 1.45 Ni 0.05 Ti 0.5 O 7-δ .

[0061] (2) SEM observation

[0062] The SEM observation was conducted using a QUANTA FEG250 scanning electron microscope (SEM) produced by FEI of the Netherlands.

[0063] Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ The observation results are as follows Figure 2 As shown, Figure 2 The results show that nanoparticles with uniform particle size have grown on the smooth substrate surface, proving that an oxide structure of RP structure doped with nickel and titanium loaded with nickel nanoparticles has been formed. 1.35 Ni 0.15 Ti 0.5 O 7-δ and Ni@Sr3Fe 1.45 Ni 0.05 Ti 0.5 O 7-δ The SEM observation results are consistent with Figure 2 Similarly, it was confirmed that an oxide structure of the RP structure doped with nickel and titanium supporting nickel nanoparticles was formed.

[0064] The application of the RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles described in this embodiment is used as an anode of a solid oxide electrolytic cell, especially as an anode of a solid oxide electrolytic cell for dehydrogenating ethane to produce ethylene; the application steps are as follows:

[0065] The mixed solution was added to 0.2 g of the RP structured oxide doped with nickel and titanium obtained in this embodiment to prepare an electrode slurry, and 0.1 g of the electrode slurry was evenly scraped on the electrolyte, calcined at 1000° C. for 5 h, and then placed in a mixed gas atmosphere of hydrogen and argon, and in-situ reduced at 800° C. for 5 h to obtain an anode on the electrolyte. The material of the anode was a porous RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles.

[0066] Wherein, the mixed solution is composed of 0.024g ethyl cellulose ([C 6+2n H 7+8n O 2+4n ] x )、0.016g soluble starch (C 12 H 22 O 11 ) and 1ml terpineol (C 10 H 18 O) mixed.

[0067] The electrolyte is yttria-stabilized zirconia coated with a transition layer, wherein the transition layer is gadolinium-doped cerium oxide (GDC), specifically 10 mol% of Gd2O3 doped CeO2, and the molar fraction of yttrium oxide in the yttria-stabilized zirconia is 8% (abbreviated as 8-YSZ).

[0068] In the mixed gas, the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0069] An electrolytic cell, wherein the electrolyte and anode of the electrolytic cell adopt the electrolyte prepared in this embodiment and the anode thereon, and the cathode material adopts NiO-YSZ, and the mass ratio of NiO to YSZ is 45:55. It is used for electrolytic dehydrogenation of ethane to produce ethylene (0V-1.8V). CO2 gas is introduced into the cathode at a total flow rate of 20ml / min, and a mixed gas of C2H6 and Ar is introduced into the anode, wherein the volume ratio of C2H6 to Ar is 1:1, the total flow rate is 20ml / min, the reaction temperature is 800°C, and a voltage is applied to both ends of the electrodes for testing using an AUTOLAB Potentiostat electrochemical workstation, such as Figure 3 As shown, when a voltage of 1.8 V is applied, when the anode material is Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δWhen the current density reaches 2.3A / cm -2 ; When the material of the anode is Ni@Sr3Fe 1.35 Ni 0.15 Ti 0.5 O 7-δ When the current density reaches 1.90A / cm -2 ; When the material of the anode is Ni@Sr3Fe 1.45 Ni 0.05 Ti 0.5 O 7-δ When the current density reaches 1.68A / cm -2 .

[0070] Example 2

[0071] A RP structured oxide (Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ), the preparation method comprising the following steps:

[0072] (1) According to Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ The contents of strontium, iron, nickel and titanium in the composition expression were calculated by weighing 6.1686 g (0.03 mol) of strontium acetate, 5.656 g (0.014 mol) of ferric nitrate, 0.29079 g (0.001 mol) of nickel nitrate and 1.6995 g (0.005 mol) of tetrabutyl titanate, and dissolving them fully in 400 ml of solvent N,N-dimethylformamide (DMF) to obtain a mixed solution.

[0073] (2) adding 10.51 g of citric acid to the mixed solution obtained in step (1), and stirring at 80° C. until a transparent yellow gel is formed;

[0074] The ratio of the total molar number of citric acid to the total molar number of metal cations in the mixed solution is 1:1.

[0075] (3) The gel prepared in step (2) is heated to 300° C. and subjected to spontaneous combustion to obtain a powder.

[0076] (4) The powder obtained in step (3) is calcined at 1100° C. for 10 h to obtain an oxide of RP structure doped with nickel and titanium.

[0077] (5) placing the RP structured oxide doped with nickel and titanium obtained in step (4) in a reducing atmosphere and treating at 800° C. for 5 h to obtain a reduced product of the RP structured oxide doped with nickel and titanium, i.e., an RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles (Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ).

[0078] Wherein, the reducing atmosphere is a mixture of hydrogen and argon, in which the volume fraction of hydrogen accounts for 20% of the volume fraction of the mixed gas.

[0079] The following tests and observations were conducted on the oxide of RP structure doped with nickel and titanium and its reduced product obtained in this embodiment:

[0080] (1) X-ray diffraction (XRD) test

[0081] The XRD test instrument used was the X'Pert PRO MPD produced by PANalytical, with a current of 40 mA, a voltage of 40 kV, a Cu target Kα ray, a scanning range of 20° to 80°, and a scanning speed of 10° min -1 .

[0082] The test results show that an XRD spectrum of an RP structure oxide doped with nickel and titanium was obtained, proving that its structural composition is Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ , a reduced product of an oxide of RP structure doped with nickel and titanium was obtained, i.e., an XRD spectrum of an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles, proving that its structural composition is Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ .

[0083] (2) SEM observation

[0084] The SEM observation was conducted using a QUANTA FEG250 scanning electron microscope (SEM) produced by FEI of the Netherlands.

[0085] The observation results showed that nanoparticles with uniform particle size grew on the smooth substrate surface, proving the formation of Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ structure.

[0086] An application of the nickel- and titanium-doped RP structured oxide loaded with nickel nanoparticles as described in this embodiment is used as an anode of a solid oxide electrolytic cell, in particular, as an anode of a solid oxide electrolytic cell for dehydrogenating ethane to produce ethylene; the application steps are as follows:

[0087] A mixed solution was added to 0.2 g of an oxide of RP structure doped with nickel and titanium obtained in this embodiment to prepare an electrode slurry, and 0.1 g of the electrode slurry was evenly scraped on the electrolyte, calcined at 1100° C. for 2 h, and then placed in a mixed gas atmosphere of hydrogen and argon, and in-situ reduced at 800° C. for 5 h to obtain an anode on the electrolyte. The material of the anode was a porous oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles.

[0088] The mixed solution is prepared by mixing 0.024 g of ethyl cellulose, 0.016 g of soluble starch and 1 ml of pinene alcohol.

[0089] The electrolyte is yttria-stabilized zirconia coated with a transition layer, wherein the transition layer is gadolinium-doped cerium oxide (GDC), specifically 10 mol% of Gd2O3 doped CeO2, and the molar fraction of yttrium oxide in the yttria-stabilized zirconia is 8% (abbreviated as 8-YSZ).

[0090] In the mixed gas, the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0091] An electrolytic cell, wherein the electrolyte and anode of the electrolytic cell adopt the electrolyte prepared in this embodiment and the anode thereon, and the cathode material adopts NiO-YSZ, and the mass ratio of NiO to YSZ is 45:55. It is used for electrolytic dehydrogenation of ethane to produce ethylene (0V-1.8V). CO2 gas is introduced into the cathode at a total flow rate of 20ml / min, and a mixed gas of C2H6 and Ar is introduced into the anode, wherein the volume ratio of C2H6 to Ar is 1:1, the total flow rate is 20ml / min, the reaction temperature is 800°C, and a voltage is applied to both ends of the electrodes for testing using an AUTOLAB Potentiostat electrochemical workstation, such as Figure 3 As shown in Figure 2, when a voltage of 1.8 V is applied, the current density reaches 2.3 A / cm -2 .

[0092] Example 3

[0093] A RP structured oxide (Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ), the preparation method comprising the following steps:

[0094] (1) According to Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ The contents of strontium, iron, nickel and titanium in the composition expression are as follows: 6.1686 g (0.03 mol) of strontium acetate, 5.656 g (0.014 mol) of iron nitrate, 0.29079 g (0.001 mol) of nickel nitrate and 1.6995 g (0.005 mol) of tetrabutyl titanate are weighed and placed in 400 ml of solvent N,N-dimethylformamide (DMF) and fully dissolved to obtain a mixed solution;

[0095] (2) adding 10.51 g of citric acid and 11.41 g of glycine to the mixed solution obtained in step (1), and stirring at 80° C. until a transparent yellow gel is formed;

[0096] The ratio of the total molar number of citric acid, glycine and metal cations in the mixed solution is 1:1:1.

[0097] (3) The gel prepared in step (2) is heated to 250° C. and subjected to spontaneous combustion to obtain a powder.

[0098] (4) The powder obtained in step (3) is calcined at 1100° C. for 6 h to obtain an oxide of RP structure doped with nickel and titanium.

[0099] (5) placing the RP structured oxide doped with nickel and titanium obtained in step (4) in a reducing atmosphere and treating at 800° C. for 5 h to obtain a reduced product of the RP structured oxide doped with nickel and titanium, i.e., an RP structured oxide doped with nickel and titanium loaded with nickel nanoparticles (Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ ).

[0100] Wherein, the reducing atmosphere is a mixture of hydrogen and argon, in which the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0101] The following tests and observations were conducted on the oxide of RP structure doped with nickel and titanium and its reduced product obtained in this embodiment:

[0102] (1) X-ray diffraction (XRD) test

[0103] The XRD test instrument used was the X'Pert PRO MPD produced by PANalytical, with a current of 40 mA, a voltage of 40 kV, a Cu target Kα ray, a scanning range of 20° to 80°, and a scanning speed of 10° min -1 .

[0104] The test results show that an XRD spectrum of an RP structure oxide doped with nickel and titanium was obtained, proving that its structural composition is Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ , a reduced product of an oxide of RP structure doped with nickel and titanium was obtained, i.e., an XRD spectrum of an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles, proving that its structural composition is Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ .

[0105] (2) SEM observation

[0106] The SEM observation was conducted using a QUANTA FEG250 scanning electron microscope (SEM) produced by FEI of the Netherlands.

[0107] The observation results showed that nanoparticles with uniform particle size grew on the smooth substrate surface, proving the formation of Ni@Sr3Fe 1.4 Ni 0.1 Ti 0.5 O 7-δ structure.

[0108] An application of the nickel- and titanium-doped RP structured oxide loaded with nickel nanoparticles as described in this embodiment is used as an anode of a solid oxide electrolytic cell, in particular, as an anode of a solid oxide electrolytic cell for dehydrogenating ethane to produce ethylene; the application steps are as follows:

[0109] A mixed solution was added to 0.2 g of an oxide of RP structure doped with nickel and titanium obtained in this embodiment to prepare an electrode slurry, and 0.1 g of the electrode slurry was evenly scraped on the electrolyte, calcined at 1200° C. for 2 h, and then placed in a mixed gas atmosphere of hydrogen and argon, and in-situ reduced at 800° C. for 5 h to obtain an anode on the electrolyte. The material of the anode was a porous oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles.

[0110] The mixed solution is prepared by mixing 0.024 g of ethyl cellulose, 0.016 g of soluble starch and 1 ml of pinene alcohol.

[0111] The electrolyte is yttria-stabilized zirconia coated with a transition layer, wherein the transition layer is gadolinium-doped cerium oxide (GDC), specifically 10 mol% of Gd2O3 doped CeO2, and the molar fraction of yttrium oxide in the yttria-stabilized zirconia is 8% (abbreviated as 8-YSZ).

[0112] In the mixed gas, the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.

[0113] An electrolytic cell, wherein the electrolyte and anode of the electrolytic cell adopt the electrolyte prepared in this embodiment and the anode thereon, and the cathode material adopts NiO-YSZ, and the mass ratio of NiO to YSZ is 45:55. It is used for electrolytic dehydrogenation of ethane to produce ethylene (0V-1.8V). CO2 gas is introduced into the cathode at a total flow rate of 20ml / min, and a mixed gas of C2H6 and Ar is introduced into the anode, wherein the volume ratio of C2H6 to Ar is 1:1, the total flow rate is 20ml / min, the reaction temperature is 800°C, and a voltage is applied to both ends of the electrodes for testing using an AUTOLAB Potentiostat electrochemical workstation, such as Figure 3 As shown in Figure 2, when a voltage of 1.8 V is applied, the current density reaches 2.3 A / cm -2 .

Claims

1. An application of an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles, characterized in that: The oxide is used as an anode of a solid oxide electrolytic cell for ethane dehydrogenation to ethylene, and the composition expression of the oxide is Ni@Sr3Fe 1.5-x Ni x Ti 0.5 O 7-δ , 0<X≤0.15, δ represents the number of randomly generated oxygen vacancies.

2. The use of an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles according to claim 1, characterized in that: Placing an oxide of RP structure doped with nickel and titanium in a reducing atmosphere and performing reduction treatment at 600° C. to 900° C. for 1 h to 20 h to obtain a reduced product of the oxide of RP structure doped with nickel and titanium, i.e., an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles; The reducing atmosphere is a mixture of hydrogen and argon, in which the volume fraction of hydrogen accounts for 5% to 20% of the volume fraction of the mixed gas; The RP structured oxide doped with nickel and titanium is formed by doping Ni and Ti in a strontium ferrite-based material, and its composition expression is Sr3Fe 1.5-x Ni x Ti 0.5 O 7-δ , 0<X≤0.15, δ represents the number of randomly generated oxygen vacancies.

3. The use of an oxide of RP structure doped with nickel and titanium loaded with nickel nanoparticles according to claim 2, characterized in that: A mixed solution prepared by mixing ethyl cellulose, soluble starch and pine alcohol is added to the above-mentioned RP structured oxide doped with nickel and titanium to prepare an electrode slurry, and the electrode slurry is evenly scraped onto an 8-YSZ electrolyte coated with a gadolinium-doped cerium oxide transition layer, calcined at 1000° C. to 1200° C. for 2 h to 5 h, and then placed in a mixture of hydrogen and argon, and in-situ reduced at 800° C. for 5 h to obtain an anode on the electrolyte, wherein the material of the anode is a porous RP structured oxide doped with nickel and titanium and loaded with nickel nanoparticles; The 8-YSZ is yttria-stabilized zirconium oxide, wherein the molar fraction of yttria is 8%; In the mixed gas, the volume fraction of hydrogen accounts for 5% of the volume fraction of the mixed gas.