A method for controlling low nitrogen content in low carbon steel
By adding scrap steel and auxiliary materials during the converter smelting process and performing top blowing and bottom blowing gas control, the nitrogen content of the steel water at the end of the converter is reduced, and the problem of difficult to control the nitrogen content in low-carbon steel is solved, and low-cost low-nitrogen steel is achieved Production meets the performance requirements of low carbon steel.
Patent Information
- Application Number
- CN202210875865.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-22
AI Technical Summary
The prior art is difficult to effectively control the nitrogen content in low carbon steel, especially when the carbon content is low, which cannot meet the requirements of low nitrogen content, which affects the performance and production process of steel.
By adding scrap steel and auxiliary materials during the converter smelting process, and performing top blowing and bottom blowing gas control, the nitrogen content of the steel water at the end of the converter is reduced, and then LF refining is carried out to achieve low nitrogen content of low carbon steel. The specific steps include in-furnace molten iron smelting , add scrap steel and auxiliary materials, and control the top and bottom blowing gas of the converter to ensure that the nitrogen content of the molten steel at the end of the converter is ≤20ppm.
It effectively reduces the nitrogen content in low carbon steel, reduces the pressure of nitrogen control in subsequent processes, reduces production costs, and improves the deep-drawing and processing performance of low carbon steel.
Smart Images

Figure CN115820971B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting, and in particular relates to a method for controlling low nitrogen content in low-carbon steel. Background Art
[0002] Except for a few types of steel, nitrogen in steel is a harmful element. The nitrogen content will reduce the plasticity of steel, affect the cold deformation processing and welding performance of steel, and cause the steel to become brittle under strain conditions, affecting the service performance of steel components. At the same time, when the nitrogen content is too high, it is easy to cause defects such as scarring and subcutaneous bubbles on the ingot, and cause linear defects or cracks on the surface of the rolled material.
[0003] The Chinese patent with patent application number 201710652781.6 discloses a method for reducing the nitrogen content of molten steel in the converter steelmaking process. The control process of the patent is: converter smelting-steel tapping control nitrogen addition; the patent can control the nitrogen content of converter molten steel below 30ppm for steel with a carbon content of 0.030%-0.050%, and control the nitrogen content in the finished steel within 50ppm. The patent mainly controls the nitrogen addition in the process after the converter tapping. At the same time, the process belongs to the control process for the production of high-nitrogen steel grades. For low-carbon steel grades with a carbon content of less than 0.030%, when the nitrogen content is required to be ≤30ppm, it cannot meet the production needs.
[0004] The Chinese patent with patent application number 201711138768.5 discloses a method for reducing the nitrogen content of molten steel at the end of the converter. The control process of the patent is as follows: loading scrap steel into the converter, with a scrap steel ratio of ≤10%; adding pellets during converter blowing, with a pellet dosage of ≥5000kg / furnace; controlling the end carbon content to ≥0.04% during converter carbon pulling, and providing molten steel with a nitrogen content of <20ppm for the refining process. This patent is mainly aimed at steel grades with a carbon content of ≥0.04% at the end of the converter, and the steel is not deoxidized during tapping, and the refining provides molten steel with a nitrogen content of <20ppm. It needs to be coordinated with the subsequent refining process to produce low-carbon steel grades. Directly using this process cannot meet the requirements for controlling the nitrogen content of low-carbon steel.
[0005] The Chinese patent with patent application number 201210487536.1 discloses a method for controlling the nitrogen content of converter steel. The control process of the patent is as follows: the molten iron requires P≤0.150%, T≥1250℃, sulfur content less than 0.015%, and the molten iron ratio is increased by 85-90%; 30-40kg / t iron ore is added during converter blowing; endpoint control C: 0.08-0.12%, P≤0.015%, S≤0.020%, T: 1650-1690℃; argon is blown from the bottom of the ladle 1-2 minutes before steel tapping, and argon is blown throughout the steel tapping process. At the same time, during the steel tapping process, the amount of bottom blowing argon is reduced for soft blowing so as not to expose the molten steel surface; two-step deoxidation is used in the steel tapping process to make the nitrogen content of the converter steel tapping 25ppm. This patent is mainly aimed at medium-carbon steels with a carbon content of 0.08%-0.12% at the converter end point, and the steelmaking is achieved using a two-step deoxidation process. However, for low-carbon steels with a carbon content of ≤0.04%, the control requirement of nitrogen content ≤20ppm cannot be achieved. Summary of the invention
[0006] The present application provides a method for controlling the low nitrogen content of low-carbon steel to solve the technical problem of high nitrogen content in low-carbon steel grades.
[0007] In a first aspect, the present application provides a method for controlling low nitrogen content in low carbon steel, the method comprising the following steps:
[0008] Smelting the molten iron into the furnace to obtain smelted molten iron;
[0009] Adding scrap steel and auxiliary materials to the smelting molten iron and performing converter top blowing to obtain converter terminal molten steel;
[0010] The converter end point molten steel is subjected to LF refining to obtain target low carbon steel to achieve a low nitrogen content of the low carbon steel, wherein the nitrogen content of the converter end point molten steel is ≤20ppm.
[0011] Optionally, in terms of mass fraction, the phosphorus content of the molten iron entering the furnace is ≤0.120%, the sulfur content of the molten iron entering the furnace is ≤0.010%, and the temperature of the molten iron entering the furnace is ≥1250°C.
[0012] Optionally, the scrap steel ratio of the scrap steel entering the furnace is ≤15%.
[0013] Optionally, the chemical components of the scrap steel include: carbon content ≤0.3%, phosphorus content ≤0.020%, sulfur content ≤0.015%, and nitrogen content ≤60ppm.
[0014] Optionally, the auxiliary material includes a first auxiliary material, the first auxiliary material includes a first lime and pellets, the first lime is added in an amount of 30-40 kg / t, and the pellets are added in an amount of 3.0-6.0 kg / t.
[0015] Optionally, the chemical components of the pellets include: TFe ≥ 62%, SiO 2 =5.0-7.0%, TiO 2 ≤0.6%、Al 2 O 3 ≤1.5%, MgO≤0.6%.
[0016] Optionally, the auxiliary material includes a second lime, and the added amount of the second lime is 3.0-5.0 kg / t.
[0017] Optionally, the second lime is added when the carbon content of the smelting molten iron is 0.25%-0.40%.
[0018] Optionally, the converter top-blown gas includes oxygen, and the converter top-blown gas has an intensity of 3.8-4.0 Nm 3 / t·min.
[0019] Optionally, the method further comprises the following steps: blowing inert gas to the bottom of the molten iron, wherein the intensity of the bottom blowing is 0.1-0.2 Nm 3 / t·min.
[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0021] The method provided in the embodiment of the present application comprises the steps of smelting molten iron into a furnace to obtain smelted molten iron; adding scrap steel and auxiliary materials to the smelted molten iron and performing top blowing of a converter to obtain molten steel at the converter end point; controlling the addition of scrap steel and auxiliary materials and performing top blowing of a converter to make the nitrogen content of the molten steel at the converter end point ≤20ppm, and controlling the nitrogen content of the molten steel at the converter end point ≤20ppm, and performing conventional control on subsequent processes including LF refining to obtain target low-carbon steel; since during conventional smelting, the molten steel contacts the air, most of the processes involve nitrogen addition, and only the vacuum process can remove part of the nitrogen, and therefore, it is necessary to control the nitrogen content in the steel through a converter to reduce the nitrogen content in the molten steel at the converter end point as much as possible, so that the carbon content of the low-carbon steel at the converter end point can be controlled at a relatively low level, so that low-carbon steel grades meet the requirements of low nitrogen content. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1 A schematic flow chart of a method for controlling low nitrogen content in low carbon steel provided in an embodiment of the present application. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0026] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. If there is a conflict, the present specification takes precedence. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. For example, room temperature can refer to a temperature within the range of 10 to 35°C.
[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0028] The technical solution of the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:
[0029] According to a typical embodiment of the present invention, a method for controlling low nitrogen content in low carbon steel is provided, such as Figure 1 As shown, the method comprises the following steps:
[0030] S1. Smelting the molten iron into the furnace to obtain molten iron;
[0031] S2. Adding scrap steel to the smelting molten iron, adding auxiliary materials and top blowing the converter to obtain the converter end point molten steel;
[0032] S3. The converter end point molten steel is subjected to LF refining to obtain target low carbon steel to achieve a low nitrogen content of the low carbon steel, wherein the nitrogen content of the converter end point molten steel is ≤20ppm.
[0033] By adding scrap steel and auxiliary materials to control the nitrogen content of the converter final molten steel to ≤20ppm, the nitrogen content in the target low-carbon steel can be effectively reduced, thereby effectively reducing the nitrogen control pressure of subsequent processes and reducing the production cost for obtaining the target low-carbon steel.
[0034] It is worth noting that for low carbon steel, the nitrogen content in the low carbon steel needs to be strictly controlled so that the low carbon steel has good deep drawing performance and processing performance and meets the performance requirements of low carbon steel.
[0035] In some embodiments, the phosphorus content of the molten iron entering the furnace is ≤0.120% by mass, the sulfur content of the molten iron entering the furnace is ≤0.010% by mass, and the temperature of the molten iron entering the furnace is ≥1250°C.
[0036] The reason for controlling the phosphorus content in the molten iron entering the furnace to ≤0.120% is to reduce the dephosphorization burden of the converter and realize the advantages of efficient and rapid dephosphorization in converter smelting; the reason for controlling the sulfur content in the molten iron entering the furnace to ≤0.010% is that the desulfurization capacity of the converter is limited, which improves favorable conditions for desulfurization in subsequent processes; the reason for controlling the temperature of the molten iron entering the furnace to ≥1250℃ is to ensure the thermal balance in the converter and have the temperature conditions required for smelting.
[0037] In some embodiments, the scrap steel ratio of the scrap steel charged into the furnace is ≤15%.
[0038] The reason for controlling the scrap steel ratio of scrap steel entering the furnace to ≤15% is the high molten iron temperature and low scrap steel ratio, which ensures that the converter molten pool has a high temperature, so that the carbon-oxygen reaction in the converter is intense, and a sufficient amount of CO can be produced to strongly stir the molten pool. At the same time, the presence of a large amount of CO in the converter reduces the partial pressure of N in the furnace, which can play a role in denitrification in the converter. If the scrap steel ratio is not within the above range, the nitrogen partial pressure in the furnace is large, which does not meet the kinetic conditions required for denitrification in the furnace, and is not conducive to the denitrification effect in the converter.
[0039] In some embodiments, the chemical composition of the scrap steel includes: carbon content ≤ 0.3%, phosphorus content ≤ 0.020%, sulfur content ≤ 0.015%, and nitrogen content ≤ 60 ppm.
[0040] In some embodiments, the auxiliary material includes a first auxiliary material, the first auxiliary material includes a first lime and pellets, the first lime is added in an amount of 30-40 kg / t, and the pellets are added in an amount of 3.0-6.0 kg / t.
[0041] The reason for controlling the addition amount of the first lime to be 30-40kg / t and the addition amount of the pellets to be 3.0-6.0kg / t is that slag is generated on the liquid surface. The slag in the converter can dephosphorize and cover the slag surface, isolate the steel liquid surface from the air, and ensure the nitrogen content control effect in the converter. If the addition amount of the first lime and the pellets is not within the above range, it will have an adverse effect on the dephosphorization and temperature control of the converter.
[0042] In some embodiments, the chemical composition of the pellets includes: TFe ≥ 62%, SiO 2 =5.0-7.0%, TiO 2 ≤0.6%、Al 2 O 3 ≤1.5%, MgO≤0.6%.
[0043] In some embodiments, the auxiliary material includes a second lime, and the added amount of the second lime is 3.0-5.0 kg / t.
[0044] The reason for controlling the addition amount of the second lime to 3.0-5.0kg / t is that the carbon content in the molten steel is relatively low at this time, the amount of CO produced is greatly reduced, and the stirring of the molten pool becomes weaker. Adding the second batch of slag can ensure that under the premise of weak stirring, the molten steel is prevented from contacting with the air and absorbing nitrogen. If the addition amount of the first lime and pelletized ore is not within the above range, it will have an adverse effect on the dephosphorization and denitrification of the converter.
[0045] In some embodiments, the second lime is added when the carbon content of the molten iron is 0.25%-0.40%.
[0046] Specifically, the timing of adding the second auxiliary material can also be when the secondary gun measures TSC when the blowing is 80%, and when the carbon content is 0.25%-0.40%, the nitrogen content of the converter for low-carbon steel smelting can be effectively controlled. The reason for adding lime when the carbon content of the smelting molten iron is 0.25%-0.40% is that it plays a role in isolating the molten steel and the atmosphere, and has the advantage of isolating the nitrogen gas supply source. If lime is added when the carbon content is not within the above range, the isolation effect is not good.
[0047] In some embodiments, the converter top-blown gas includes oxygen, and the converter top-blown gas has an intensity of 3.8-4.0 Nm 3 / t·min.
[0048] Control the top blowing strength of the converter to 3.8-4.0Nm 3 / t·min is due to the top and bottom combined blowing of the converter, which ensures the stirring effect of the molten pool and provides good dynamic conditions for dephosphorization and denitrification. If the intensity of the converter top blowing is not within the above range, it will have the adverse effects of unreasonable stirring intensity and unsatisfactory dynamic conditions.
[0049] In some embodiments, the method further comprises the following steps: blowing inert gas to the bottom of the molten iron, wherein the flow rate of the bottom blowing is 0.1-0.2 Nm 3 / t·min.
[0050] Specifically, the inert gas includes but is not limited to argon, and the flow rate of the bottom blowing is controlled to be 0.1-0.2Nm 3 The reason for the value of / t·min is to ensure the kinetic conditions required for denitrification, which has the advantage of converter denitrification kinetics. If the bottom blowing flow rate is not within the above range, it will have the adverse effect of not meeting the denitrification kinetic conditions.
[0051] The method of the present invention will be described in detail below with reference to embodiments, comparative examples and experimental data.
[0052] Example 1
[0053] This embodiment provides a method for controlling low nitrogen content in low carbon steel. Figure 1 As shown, the method comprises the following steps:
[0054] S1. Smelting the molten iron into the furnace to obtain molten iron;
[0055] S2. adding scrap steel and auxiliary materials to the smelting molten iron and performing top blowing of the converter to obtain converter terminal molten steel to achieve a low nitrogen content in low-carbon steel.
[0056] Specifically include:
[0057] Control the molten iron entering the converter, requiring the composition of the molten iron to be [P] = 0.120%, [S] = 0.010%, and the temperature of the molten iron to be T = 1250°C; at the same time, control the scrap steel ratio entering the converter, which is 15%. The amount of lime added to the first batch of converter smelting is 30kg / t steel, the pellet ore is 4kg / t steel, the converter top-blown oxygen, and the top-blowing intensity is 4.0Nm 3 / t·min; and the whole process of bottom blowing argon is adopted, and the bottom blowing argon intensity is controlled to 0.1Nm 3 / t·min, TSC measurement was carried out using an auxiliary lance when the converter was blowing 80%, and the carbon content at this time was controlled to be 0.40%. The second batch of lime was added into the converter for slagging, and the added amount was 3kg / t steel.
[0058] Through the above converter process control technology, the carbon content at the converter end point is controlled to 0.040%, and the nitrogen content at the converter end point is controlled to 18ppm.
[0059] Example 2
[0060] The difference between this embodiment and embodiment 1 is that: the molten iron fed into the converter is controlled, and the composition of the molten iron is required to be [P]=0.090%, [S]=0.008%, and the temperature of the molten iron is T=1300°C; at the same time, the scrap steel ratio fed into the converter is controlled, and the scrap steel ratio fed into the converter is 13%; the amount of lime added to the first batch of converter smelting is 40kg / t steel, and the pellet ore is 6kg / t steel; oxygen is top-blown in the converter, and the top-blowing intensity is 3.8Nm 3 / t·min; and the whole process of bottom blowing argon is adopted, and the bottom blowing argon intensity is controlled to 0.2Nm 3 / t·min, the top and bottom of the converter are blown together to ensure the stirring effect of the molten pool and provide good dynamic conditions for dephosphorization and denitrification. When the converter is 80% blown, TSC measurement is carried out using the auxiliary gun. At this time, the carbon content is controlled to be 0.250%. The second batch of lime is added to the converter for slagging, and the addition amount is 5kg / t steel.
[0061] Through the above converter process control technology, the carbon content at the converter end point is controlled to 0.025%, and the nitrogen content at the converter end point is controlled to 14ppm.
[0062] Comparative Example 1
[0063] The difference between the comparative example of the present application and Example 1 is that:
[0064] Compared with the technology with patent application number 201711138768.5, it mainly controls the nitrogen content by controlling the nitrogen addition in the process after the converter steel is tapped; this process belongs to the control process for the production of high-nitrogen steel grades. For low-carbon steel grades with a carbon content of less than 0.030% when the nitrogen content is required to be ≤30ppm, it cannot meet the production needs; at the same time, there is no description of the amount of auxiliary materials added to the converter smelting, and the top blowing and bottom blowing control process parameters of the converter.
[0065] Comparative Example 2
[0066] The difference between the comparative example of the present application and Example 1 is that:
[0067] In comparison, the technology with patent application number 201711138768.5 is mainly aimed at steel with a carbon content ≥0.04% at the converter end point, and the steel is not deoxidized during tapping. The refining provides molten steel with a nitrogen content of <20ppm. It needs to be coordinated with subsequent refining steps to produce low-carbon steel grades. Directly using this process cannot meet the requirements for controlling the nitrogen content of low-carbon steel. At the same time, it does not explain the amount of auxiliary materials added to the converter smelting, and the top blowing and bottom blowing control process of the converter.
[0068] Comparative Example 3
[0069] The difference between the comparative example of the present application and Example 1 is that:
[0070] In comparison, the technology with patent application number 201210487536.1 is mainly aimed at medium-carbon steels with a carbon content of 0.08%-0.12% at the converter end point, and the steelmaking is achieved by a two-step deoxidation process. For low-carbon steels with a carbon content of ≤0.04%, the control requirement of nitrogen content ≤20ppm cannot be achieved; at the same time, it does not explain the amount of auxiliary materials added to the converter smelting, and the top blowing and bottom blowing control process of the converter.
[0071] It can be seen from the embodiments and comparative examples that different production processes can achieve different effects on the control of the nitrogen content of low carbon steel, and bring about different economic values and costs, as shown in Table 1.
[0072]
[0073]
[0074] The alloy is a manganese alloy added at the end of the converter. Different types of alloys are added according to the different molten steel at the end of the converter. The costs of different alloys are different, as shown in the table. Note: The patented process control technology can achieve low nitrogen content control at the end of the converter. Therefore, low-cost low-nitrogen steel production can be achieved, which reflects the low-cost effect from two aspects: 1) shortening the process control cost of nitrogen content in subsequent processes; 2) the low nitrogen content at the end of the converter allows ordinary alloys to be used in subsequent smelting processes instead of low-nitrogen alloys, reducing alloy costs. The calculation is based on a steel containing 1.2% Mn as an example.
[0075] As can be seen from the table, the embodiment groups 1 and 2, and the comparative example groups 1, 2, and 3, the embodiment groups can more accurately control the nitrogen content than the comparative examples, and can achieve the effect of cost saving.
[0076] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "including a..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.
[0077] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for controlling low nitrogen content in low carbon steel. It is characterized in that The method comprises the following steps: controlling the molten iron fed into the converter, wherein the composition of the molten iron is [P]=0.090%, [S]=0.008%, and the temperature of the molten iron is T=1300°C; controlling the scrap steel ratio fed into the converter, wherein the scrap steel ratio is 13%; adding 40kg / t steel and 6kg / t steel of pellets to the first batch of smelting in the converter; top blowing oxygen into the converter, wherein the top blowing intensity is 3.8Nm 3 / t·min; and the whole process of bottom blowing argon is adopted, and the bottom blowing argon intensity is controlled to 0.2Nm 3 / t·min, TSC measurement was carried out with an auxiliary lance when the converter was blowing 80%, and the carbon content at this time was controlled at 0.250%. The second batch of lime was added into the converter for slagging, and the added amount was 5kg / t steel; the carbon content at the converter end point was controlled at 0.025%, and the nitrogen content at the converter end point was controlled at 14ppm.
Citation Information
Cited By
Molten steel and method preparing the same
TWI934744B