Conductive dry-process acrylic fiber and preparation method thereof

By treating the nascent acrylic filaments with an alkaline solution and dispersing them with graphene, the problems of static electricity and uneven dispersion of conductive acrylic fibers in textiles were solved, and conductive acrylic fibers with high conductivity and good spinnability were prepared.

CN115821573BActive Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111086916.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-16
Publication Date
2024-11-15
Estimated Expiration
2041-09-16
Patent Text Reader

Abstract

A method for preparing conductive dry-process acrylic primary yarn, and conductive dry-process acrylic primary yarn and conductive dry-process acrylic fiber prepared by the method. The preparation method comprises: pre-treating the acrylic primary yarn with an alkaline solution to obtain the pre-treated acrylic primary yarn with a porosity of 20 to 30% by volume; grinding graphene into graphene powder and preparing a graphene dispersion with a certain concentration; slowly passing the pre-treated acrylic primary yarn through the graphene dispersion to load the graphene on the acrylic primary yarn; and finally using a curing agent to stably load the graphene on the surface of the acrylic primary yarn to obtain the conductive dry-process acrylic primary yarn. The prepared conductive dry-process acrylic fiber has good spinnability and conductivity, and a simple manufacturing process, which saves production time and cost and is easy for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of dry-process acrylic fibers, and in particular relates to conductive dry-process acrylic fibers and a preparation method thereof. Background Art

[0002] Acrylic is the trade name of polyacrylonitrile fiber in my country. It has high elasticity, strength, heat resistance, light resistance and corrosion resistance, and is widely used in the textile industry. Because of its bright color, light and soft texture, and its appearance and feel are similar to wool, it is called "synthetic wool".

[0003] The polyacrylonitrile (PAN) macromolecules in acrylic fiber contain a large number of hydrophobic groups, which makes acrylic fiber highly hydrophobic and extremely poor in hygroscopicity, making it very easy to generate static electricity, which further leads to the generation of static electricity due to friction and induction during the production, processing and use of textiles. The resistivity of conventional fiber materials is above 1010Ω.cm, and the generated charge is not easy to dissipate, which often causes the static-carrying fibers to entangle or block the machine parts; and the warp opening is unclear and the fabric is unevenly folded during weaving, which seriously affects the smooth progress of production. Furthermore, during the use of acrylic textiles, the accumulation of static electricity is easy to cause dust adhesion, causing clothing to entangle limbs, easily causing adhesion discomfort, and can cause physiological changes such as increased blood pH, all of which greatly reduce the wearing performance of acrylic textiles. In addition, the higher potential generated by static electricity may also cause electric shock to the human body, and may also break down electronic components and cause damage to electronic components; the electromagnetic radiation generated by electrostatic discharge will cause electromagnetic interference to various electronic equipment and information systems.

[0004] In order to eliminate static electricity in acrylic fibers and their products, promote the rapid development of acrylic production, and meet people's growing demand for high-quality fibers and fabrics, people began to seek methods to modify the conductive properties of acrylic fibers to enhance their antistatic properties and improve their wearing comfort.

[0005] In the existing technology, the development of antistatic technology for textile materials has gone through three stages:

[0006] (1) Use surfactants to hydrophilize fibers or fabrics to increase the hygroscopicity of the fibers, thereby reducing the resistivity of the textiles and accelerating charge dissipation. However, the antistatic effect of this method is difficult to preserve for a long time, and it is easy to cause acrylic fibers to have poor washing resistance and not show antistatic properties in a low humidity environment.

[0007] (2) Antistatic fibers are prepared by introducing hydrophilic polar groups into fiber-forming polymers through blending, copolymerization, and grafting, or by adding antistatic agents into the fibers. Since the resistivity of antistatic fibers is 108-1010Ω·cm, textiles made of antistatic fibers or mixed with ordinary synthetic fibers in a high proportion can eliminate static electricity problems during processing and use. However, a high humidity environment is still a necessary condition for charge dissipation, which limits its application.

[0008] (3) Research and development of conductive fibers. The research on conductive fibers mainly includes the research on uniform conductive fibers made of conductive materials such as metal fibers, carbon fibers, and conductive polymers; or the research on coated conductive fibers obtained by coating the outer layer of synthetic fibers with conductive materials such as carbon black. According to research, the resistivity of conductive fibers obtained by composite spinning of carbon black or metal compounds and fiber-forming polymers is generally less than 10 -7 Ω·cm, even as small as 10 -4 ~10 -5 Ω·cm. The development and application of conductive fibers make the antistatic effect of the textiles made significant, and the conductive effect is durable and not affected by the environmental humidity. It can also be used in special functional textiles such as antistatic work clothes.

[0009] However, after the conductive additives used in the existing conductive fibers are applied to textiles, additives such as carbon black are generally insoluble in solvents, and the polyacrylonitrile solution prepared during spinning has a high viscosity. Therefore, when preparing the polyacrylonitrile solution, the conductive additives tend to clump together, which further leads to uneven dispersion of the additives in the final formed fibers. At the same time, the added additives will make the molecular chains in the fibers rigid, which ultimately leads to low strength, brittleness, easy breakage and other problems in the finished fibers, making it impossible to use the fibers for downstream finished products.

[0010] The prior art CN107245878A discloses a method for improving the preparation of acrylic fiber, but there is a problem with this method, that is, it does not process the graphene, and does not configure a suitable dispersion liquid, which will cause the graphene to agglomerate and precipitate. It has to be prepared and used immediately, and it is easy to precipitate during transportation. Agglomerates are easy to appear during the spinning process, resulting in poor distribution on the fiber.

[0011] Therefore, there is an urgent need for a new conductive dry-process acrylic fiber with high conductivity and excellent performance and a preparation method thereof to solve the above technical problems. Summary of the invention

[0012] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a conductive dry-process acrylic fiber with high conductivity and excellent performance and a preparation method thereof. The obtained acrylic fiber has good conductivity and excellent processing performance, and can be used to manufacture special clothing with good hand feel and comfortable wearing.

[0013] To achieve the above object, the present invention provides the following technical solutions:

[0014] The present invention provides a method for preparing conductive dry-process acrylic primary yarn, comprising the following steps:

[0015] (1) Pretreatment of dry-spun acrylic primary yarn: using an alkaline solution at a certain concentration and temperature to pretreat the acrylic primary yarn, so that a certain number of small pores appear on the surface of the pretreated dry-spun acrylic primary yarn, and the porosity is 20 to 30% by volume;

[0016] (2) Graphene pretreatment: grinding graphene into graphene powder with a certain particle size to facilitate loading graphene onto acrylic primary yarn;

[0017] (3) Preparation of graphene dispersion: adding the graphene powder pretreated in step (2) to an aqueous dispersion containing polyethylene glycol, mixing using a dispersing device, and preparing a graphene dispersion having a certain concentration;

[0018] (4) graphene preloading: passing the pretreated acrylic spun yarn obtained in step (1) through a bath containing the graphene dispersion described in step (3) at a certain pulling speed, and loading the graphene onto the surface of the acrylic spun yarn and into the small pores formed on the surface when the acrylic spun yarn passes through the bath;

[0019] (5) Graphene curing treatment: The acrylic primary yarn loaded with graphene is passed through a bath containing a curing agent solution at a certain pulling speed to thoroughly and stably load the graphene onto the surface of the acrylic primary yarn, thereby finally preparing a conductive dry-process acrylic primary yarn.

[0020] Wherein, in the step (1), the alkaline solution is a sodium hydroxide or potassium hydroxide solution, the concentration of which is 8 to 12 wt %, the temperature of the alkaline solution is 60 to 80° C., and the pretreatment time is 4 to 8 h.

[0021] Wherein, in the step (1), the alkaline solution is preferably sodium hydroxide, with a concentration of 10wt%, a temperature of 75°C, and a pretreatment time of 6h.

[0022] Wherein, in the step (2), the graphene is ground by a ball mill to obtain spherical graphene powder with a certain particle size.

[0023] Wherein, in the step (2), the graphene is one or more of single-layer graphene, few-layer graphene or graphene oxide.

[0024] Wherein, in the step (2), the ground graphene powder has a particle size of 15 to 25 μm.

[0025] Wherein, in the step (3), the molecular weight of the polyethylene glycol is 8000-10000, preferably 8000-9000.

[0026] Wherein, in the step (3), the method for preparing the graphene dispersion comprises:

[0027] (a) adding polyethylene glycol to water, stirring at 80-90° C. and 700-900 rpm (preferably 600-800 rpm) to prepare an aqueous solution with a concentration of 5-7 wt %, wherein the rotational viscosity of the solution is 600-1000 mPa.s, which is conducive to uniform dispersion of graphene without precipitation;

[0028] (b) adding the graphene powder obtained in step (2) to the aqueous solution prepared in step (a), dispersing the graphene powder into the aqueous solution under the action of a high-speed shearing machine, with a shear rate of 8000 to 10000 rpm and a shear time of 3 to 5 min to obtain a uniformly dispersed graphene dispersion, wherein the concentration of the graphene powder is 3 to 10 wt %.

[0029] Wherein, in step (4), the bathtub is a rectangular structure with a length of 9-11 m (preferably 10-11 m) and a depth of 0.5-1.5 m (preferably 1-1.5 m).

[0030] Wherein, in the step (4), the drawing speed of the acrylic primary yarn is 0.2-0.5 m / min, preferably 0.3 m / min.

[0031] Wherein, in the step (5), the curing agent is one or more of ethylenetriamine, diethylenetriamine, triethylenetetramine, preferably triethylenetetramine, preferably ethylenetriamine, or preferably a mixture of ethylenetriamine and diethylenetriamine. 。

[0032] Wherein, in the step (5), the concentration of the curing agent solution is 5 to 7 wt%.

[0033] Wherein, in the step (5), the curing temperature is 70-90° C., and the drawing speed of the acrylic primary yarn is 0.6-0.8 m / min.

[0034] The present invention also provides conductive dry-process acrylic primary yarn prepared by the method for preparing the conductive dry-process acrylic primary yarn.

[0035] The present invention also provides a method for preparing conductive dry-process acrylic fiber, wherein after step (5) of the method for preparing the conductive dry-process acrylic fiber spun yarn, step (6) is further performed: the conductive dry-process acrylic fiber spun yarn obtained by step (5) is subjected to a subsequent process to obtain the conductive dry-process acrylic fiber, and the subsequent process includes drawing, curling, and oiling.

[0036] The present invention also provides conductive dry-process acrylic fiber prepared by the conductive dry-process acrylic fiber preparation method.

[0037] The present invention has the following beneficial technical effects:

[0038] (1) The present invention provides a method for preparing conductive dry-spun acrylic fiber, which enables the dry-spun acrylic fiber to have good conductivity by loading graphene on the surface of the dry-spun acrylic fiber primary yarn.

[0039] (2) Since the surface of dry-process acrylic fiber is relatively smooth and has almost no pores, if the conductive material is loaded onto the acrylic fiber surface by ordinary dipping, spraying, etc., the conductive material loaded on the surface is very easy to detach during subsequent processing and use, thus quickly making the acrylic fiber non-conductive. However, the present method firstly causes a hydrolysis and etching reaction on the surface of the dry-process acrylic fiber primary yarn by treating it with an alkaline solution, and a large number of tiny channels appear on the surface of the acrylic fiber primary yarn, which is conducive to loading graphene particles in the channels.

[0040] (3) The preparation method of the present invention also processes the graphene material into powder particles that are smaller than the diameter of the tiny pores on the surface of the acrylic primary yarn, which is more conducive to the graphene material entering the pores.

[0041] (4) In order to facilitate the graphene powder particles to enter the micro-pores on the surface of the acrylic primary yarn, the present invention also prepares the graphene powder into a graphene dispersion. In the process of preparing the graphene dispersion, since the graphene has been treated and the powder particle size is relatively small, it is easy to clump and precipitate in the aqueous solution. In order to solve this problem, the present invention controls the solution viscosity of the graphene dispersion within a certain range, and at the same time performs high-speed shear treatment on the graphene dispersion, so that the graphene can be uniformly dispersed in the aqueous solution, thereby reducing the problems of graphene clumping and precipitation, and facilitating the subsequent graphene loading.

[0042] (5) After the graphene material is loaded into the pores, the preparation method of the present invention adopts a curing process to prevent the graphene material from falling off during subsequent processing and use. By selecting a suitable curing agent and curing process, the graphene that has entered the acrylic pores and is loaded on the surface is cured onto the fiber, thereby preparing conductive acrylic primary yarn with durable conductivity.

[0043] (6) The conductive dry-spun acrylic fiber of the present invention has good spinnability and makes the dry-spun acrylic fiber conductive without affecting the mechanical properties of the fiber. The specific resistivity is between 1.5 and 3×10 3 (Ω·cm), and at the same time, the present invention simplifies the manufacturing process of the conductive acrylic fiber, saves production time, and is easy for industrial production. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] Example 1

[0046] (1) Pretreatment of dry-spun acrylic spun yarn: The surface of the acrylic spun yarn was treated with a sodium hydroxide solution having a concentration of 8% and a temperature of 60°C for 4 hours. A certain number of small pores appeared on the surface of the dry-spun acrylic spun yarn after pretreatment, and the porosity was 23.8% by volume.

[0047] (2) Graphene pretreatment: The graphene oxide was ground using a ball mill, and the average particle size after treatment was 15 μm;

[0048] (3) Preparation of graphene dispersion: polyethylene glycol with a molecular weight of 8000 was added to water, and a 5% aqueous solution was prepared at a temperature of 80° C. and a stirring speed of 800 rpm. The solution had a rotational viscosity of 600 mPa.s. The pretreated graphene powder was then added to the above solution, and the graphene was dispersed in the aqueous solution under the action of a high-speed shearing machine at a shear rate of 8000 rpm and a shear time of 3 min to obtain a uniformly dispersed graphene dispersion with a graphene concentration of 3%.

[0049] (4) Preparation of conductive acrylic spun yarn: The pretreated acrylic spun yarn was passed through a bath containing a graphene dispersion at a pulling speed of 0.2 m / min, and then the spun yarn loaded with graphene was passed through a bath containing a vinyltriamine aqueous solution at a pulling speed of 0.6 m / min. The concentration of the curing agent solution was 5%, and the curing temperature was 70° C., finally obtaining conductive acrylic spun yarn;

[0050] (5) Preparation of conductive acrylic fiber: The prepared conductive acrylic fiber spun yarn is subjected to subsequent preparation processes such as drawing, curling, and oiling to finally obtain a conductive acrylic finished product.

[0051] Example 2

[0052] (1) Pretreatment of dry-spun acrylic spun yarn: The acrylic fiber was surface treated with a sodium hydroxide solution with a concentration of 12% and a temperature of 80°C for 8 hours. After the pretreatment, a certain number of small pores appeared on the surface of the dry-spun acrylic spun yarn, and the porosity was 26.4% by volume. ;

[0053] (2) Graphene pretreatment: The graphene oxide was ground using a ball mill, and the average particle size after treatment was 25 μm;

[0054] (3) Preparation of graphene dispersion: polyethylene glycol with a molecular weight of 8000 was added to water, and a 7% aqueous solution was prepared at a temperature of 90° C. and a stirring speed of 800 rpm. The solution had a rotational viscosity of 1000 mPa.s. The treated graphene was then added to the above solution, and the graphene was dispersed in the aqueous solution under the action of a high-speed shearing machine at a shear rate of 8000 rpm and a shear time of 5 min to obtain a uniformly dispersed graphene dispersion with a graphene concentration of 10%.

[0055] (4) Preparation of conductive acrylic spun yarn: The pretreated acrylic spun yarn was passed through a bath containing a graphene dispersion at a pulling speed of 0.5 m / min, and then the spun yarn loaded with graphene was passed through a bath containing a vinyltriamine aqueous solution at a pulling speed of 0.8 m / min. The concentration of the curing agent solution was 7%, and the curing temperature was 90° C., finally obtaining conductive acrylic spun yarn;

[0056] (5) Preparation of conductive acrylic fiber: The prepared conductive acrylic fiber spun yarn is subjected to subsequent preparation processes such as drawing, curling, and oiling to finally obtain a conductive acrylic finished product.

[0057] Example 3

[0058] (1) Pretreatment of dry-spun acrylic spun yarn: The acrylic fiber was surface treated with a potassium hydroxide solution having a concentration of 10% and a temperature of 70°C for 6 hours. A certain number of small pores appeared on the surface of the dry-spun acrylic spun yarn after pretreatment, and the porosity was 29.2% by volume.

[0059] (2) Graphene pretreatment: The graphene oxide was ground using a ball mill, and the average particle size after treatment was 20 μm;

[0060] (3) Preparation of graphene dispersion: polyethylene glycol with a molecular weight of 8000 was added to water, and a 6% aqueous solution was prepared at a temperature of 85° C. and a stirring speed of 800 rpm. The solution had a rotational viscosity of 752 mPa.s. The treated graphene was then added to the above solution, and the graphene was dispersed in the aqueous solution under the action of a high-speed shearing machine at a shear rate of 8000 rpm and a shear time of 4 min to obtain a uniformly dispersed graphene dispersion with a graphene concentration of 8%;

[0061] (4) Preparation of conductive acrylic spun yarn: The pretreated acrylic spun yarn was passed through a bath containing a graphene dispersion at a pulling speed of 0.4 m / min, and then the spun yarn loaded with graphene was passed through a bath containing a vinyltriamine aqueous solution at a pulling speed of 0.7 m / min. The concentration of the curing agent solution was 6%, and the curing temperature was 80° C., finally obtaining conductive acrylic spun yarn;

[0062] (5) Preparation of conductive acrylic fiber: The prepared conductive acrylic fiber spun yarn is subjected to subsequent preparation processes such as drawing, curling, and oiling to finally obtain a conductive acrylic finished product.

[0063] Example 4

[0064] (1) Pretreatment of dry-spun acrylic spun yarn: The acrylic fiber was surface treated with a potassium hydroxide solution with a concentration of 11% and a temperature of 65°C for 5 h. After the pretreatment, a certain number of small pores appeared on the surface of the dry-spun acrylic spun yarn, and the porosity was 22.3%.

[0065] (2) Graphene pretreatment: The graphene oxide was ground using a ball mill, and the average particle size after treatment was 15 μm;

[0066] (3) Preparation of graphene dispersion: polyethylene glycol with a molecular weight of 8000 was added to water, and a 6% aqueous solution was prepared at a temperature of 80° C. and a stirring speed of 800 rpm. The solution had a rotational viscosity of 672 mPa.s. The treated graphene was then added to the above solution, and the graphene was dispersed in the aqueous solution under the action of a high-speed shearing machine at a shear rate of 8000 rpm and a shear time of 4 min to obtain a uniformly dispersed graphene dispersion with a graphene concentration of 7%.

[0067] (4) Preparation of conductive acrylic spun yarn: The pretreated acrylic spun yarn was passed through a bath containing a graphene dispersion at a pulling speed of 0.2 m / min, and then the spun yarn loaded with graphene was passed through a bath containing a diethylenetriamine aqueous solution at a pulling speed of 0.6 m / min. The concentration of the curing agent solution was 7%, and the curing temperature was 70° C., finally obtaining conductive acrylic spun yarn;

[0068] (5) Preparation of conductive acrylic fiber: The prepared conductive acrylic fiber spun yarn is subjected to subsequent preparation processes such as drawing, curling, and oiling to finally obtain a conductive acrylic finished product.

[0069] Example 5

[0070] (1) Pretreatment of dry-spun acrylic spun yarn: The acrylic fiber was surface treated with a sodium hydroxide solution having a concentration of 11% and a temperature of 75°C for 4 hours. A certain number of small pores appeared on the surface of the dry-spun acrylic spun yarn after pretreatment, and the porosity was 23.8%.

[0071] (2) Graphene pretreatment: The graphene oxide was ground using a ball mill, and the average particle size after treatment was 22 μm;

[0072] (3) Preparation of graphene dispersion: polyethylene glycol with a molecular weight of 8000 was added to water, and a 7% aqueous solution was prepared at a temperature of 80° C. and a stirring speed of 800 rpm. The solution rotational viscosity was 953 mPa.s. The treated graphene was then added to the above solution, and the graphene was dispersed in the aqueous solution under the action of a high-speed shearing machine at a shear rate of 8000 rpm and a shear time of 3 min to obtain a uniformly dispersed graphene dispersion with a graphene concentration of 6%.

[0073] (4) Preparation of conductive acrylic spun yarn: The pretreated acrylic spun yarn was passed through a bath containing a graphene dispersion at a pulling speed of 0.2 m / min, and then the spun yarn loaded with graphene was passed through a bath containing a vinyltriamine aqueous solution at a pulling speed of 0.6 m / min. The concentration of the curing agent solution was 7%, and the curing temperature was 70° C., finally obtaining conductive acrylic spun yarn;

[0074] (5) Preparation of conductive acrylic fiber: The prepared conductive acrylic fiber spun yarn is subjected to subsequent preparation processes such as drawing, curling, and oiling to finally obtain a conductive acrylic finished product.

[0075] The conductivity of the conductive acrylic fibers obtained in Examples 1-5 was tested according to GB / T 14342-2015, and the results are shown in Table 1.

[0076] Table 1 Conductivity of the conductive acrylic fibers obtained in Examples 1-5

[0077] Example Unwashed specific resistance (Ω·cm) Specific resistance after 50 washes (Ω·cm) Example 1 <![CDATA[1.5×10 3 ]]> <![CDATA[3×10 3 ]]> Example 2 <![CDATA[1.7×10 3 ]]> <![CDATA[4×10 3 ]]> Example 3 <![CDATA[3×10 3 ]]> <![CDATA[5×10 3 ]]> Example 4 <![CDATA[2.7×10 3 ]]> <![CDATA[4.6×10 3 ]]> Example 5 <![CDATA[2.5×10 3 ]]> <![CDATA[4.3×10 3 ]]>

[0078] Comparative Example 1:

[0079] A modified acrylic fiber, comprising the following specific steps:

[0080] 200 g of graphene and 2 kg of acrylic fiber slices were melt-granulated to obtain graphene composite acrylic fiber masterbatch;

[0081] The graphene composite acrylic masterbatch was mixed with 13 kg of acrylic chips and then melt-spun to obtain modified acrylic fibers.

[0082] The obtained fiber was tested according to GB / T 14342-2015, and its specific resistivity without washing was 1×10 13 Ω·cm.

[0083] Comparative Example 2

[0084] A modified acrylic fiber is modified by impregnation at room temperature, and the specific steps are:

[0085] A graphene dispersion is prepared, wherein the particle size of the graphene in the graphene dispersion is between 0.1 and 3 μm; acrylic fiber is immersed in the graphene dispersion at 25° C. for 30 minutes, then taken out and dried to obtain modified acrylic fiber.

[0086] The obtained fiber was tested according to GB / T 14342-2015, and its specific resistivity without washing was 1×10 4 Ω·cm, the specific resistance after washing 20 times is 1×10 10 Ω·cm.

[0087] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing conductive dry-process acrylic primary yarn, comprising the following steps: (1) Pretreatment of dry-spun acrylic primary yarn: using an alkaline solution at a certain concentration and temperature to pretreat the acrylic primary yarn, so that a certain number of small pores appear on the surface of the pretreated dry-spun acrylic primary yarn, and the porosity is 20 to 30% by volume; (2) Graphene pretreatment: grinding graphene into graphene powder with a certain particle size to facilitate loading graphene onto acrylic primary yarn; (3) Preparation of graphene dispersion: adding the graphene powder pretreated in step (2) to an aqueous dispersion containing polyethylene glycol, mixing using a dispersing device, and preparing a graphene dispersion having a certain concentration; (4) graphene preloading: passing the pretreated acrylic spun yarn obtained in step (1) through a bath containing the graphene dispersion described in step (3) at a certain pulling speed, and loading the graphene onto the surface of the acrylic spun yarn and into the small pores formed on the surface when the acrylic spun yarn passes through the bath; (5) Graphene curing treatment: The acrylic primary yarn loaded with graphene is passed through a bath containing a curing agent solution at a certain pulling speed to thoroughly and stably load the graphene on the surface of the acrylic primary yarn, and finally a conductive dry-process acrylic primary yarn is prepared; Wherein, in the step (1), the alkaline solution is a sodium hydroxide or potassium hydroxide solution, the concentration of which is 8 to 12 wt%, the temperature of the alkaline solution is 60 to 80°C, and the pretreatment time is 4 to 8 hours; Wherein, in the step (2), the graphene powder after grinding has a particle size of 15 to 25 μm; Wherein, in the step (3), the concentration of graphene powder in the graphene dispersion is 3 to 10 wt%; Wherein, in the step (5), the curing agent is one or more of ethylenetriamine, diethylenetriamine, and triethylenetetramine.

2. The method for preparing conductive dry-process acrylic primary yarn according to claim 1, wherein: In the step (2), the graphene is one or more of single-layer graphene, few-layer graphene or graphene oxide.

3. The method for preparing conductive dry-process acrylic primary yarn according to claim 1, wherein: In the step (3), the method for preparing the graphene dispersion comprises: (a) adding polyethylene glycol to water, stirring at 80-90° C. and 700-900 rpm to prepare an aqueous solution with a concentration of 5-7 wt %, wherein the rotational viscosity of the solution is 600-1000 mPa.s, which is conducive to uniform dispersion of graphene without precipitation; (b) adding the graphene powder obtained in step (2) to the aqueous solution prepared in step (a), dispersing the graphene powder into the aqueous solution under the action of a high-speed shearing machine, with a shear rate of 8000 to 10000 rpm and a shear time of 3 to 5 min to obtain a uniformly dispersed graphene dispersion, wherein the concentration of the graphene powder is 3 to 10 wt %.

4. The method for preparing conductive dry-process acrylic primary yarn according to claim 1, wherein: In the step (5), the curing temperature is 70 to 90° C., and the concentration of the curing agent solution is 5 to 7 wt %.

5. The method for preparing conductive dry-process acrylic primary yarn according to claim 1, wherein: In the step (5), the curing temperature is 70-90° C., and the drawing speed of the acrylic primary yarn is 0.6-0.8 m / min.

6. The method for preparing conductive dry-process acrylic primary yarn according to claim 1 or 3, wherein: In the step (3), the molecular weight of the polyethylene glycol is 8000-10000.

7. The method for preparing conductive dry-process acrylic primary yarn according to claim 1, wherein: In the step (5), the curing agent is ethylenetriamine, or a mixture of ethylenetriamine and diethylenetriamine.

8. A conductive dry-spun acrylic primary yarn, prepared by the method for preparing conductive dry-spun acrylic primary yarn according to any one of claims 1 to 7.

9. A method for preparing conductive dry-spun acrylic fiber, comprising the method for preparing conductive dry-spun acrylic fiber spun yarn according to any one of claims 1 to 7, and after step (5) of the method for preparing conductive dry-spun acrylic fiber spun yarn according to any one of claims 1 to 7, further performing step (6): subjecting the conductive dry-spun acrylic fiber spun yarn obtained by step (5) to a subsequent process to obtain the conductive dry-spun acrylic fiber, wherein the subsequent process comprises stretching, curling, and oiling.