Self-closing pore moisture-retaining curing membrane and preparation method thereof and application in concrete curing

The self-impressive pore moisturizing and curing film prepared by electrospinning uses nanofiber hydrophobic layer and swelling layer to reduce moisture evaporation. Combined with the permeable non-woven protective layer, it is convenient to lay and rehydrate the existing film thickness and complex process. Problem, improving the early strength and frost resistance of concrete.

CN115847931BActive Publication Date: 2024-11-22YANGTZE THREE GORGES TECHNOLOGY & ECONOMY DEVELOPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211482847.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-22
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

The water-absorbing particles in the existing moisturizing and curing films lead to large film thickness, complex laying process and inability to rehydrate, which has problems of moisture volatility and environmental pollution.

Method used

Using a self-closed pore moisturizing and curing film composed of nanofiber hydrophobic layer, nanofiber swelling layer and permeable non-woven fabric, it is prepared by electrospinning process. The hydrophobic properties and structure of the nanofiber hydrophobic layer and swelling layer reduce moisture evaporation, and the protective layer is protected. Easy to rehydrate later.

Benefits of technology

The film thickness, convenient laying and secondary water replenishment are achieved, which reduces moisture volatility, improves the early strength and frost resistance of concrete, and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115847931B_ABST
    Figure CN115847931B_ABST
Patent Text Reader

Abstract

The present invention provides a self-closed pore moisturizing curing membrane and a preparation method thereof and application in concrete curing. The curing membrane comprises a moisturizing layer, a nanofiber hydrophobic layer, a nanofiber swelling layer and a protective layer arranged in sequence from bottom to top; wherein the moisturizing layer and the protective layer are non-woven fabrics; the nanofiber hydrophobic layer is formed by spinning after a hydrophobic polymer is dissolved in a solvent and hydrophobic nanoparticles are added, and the nanofiber swelling layer is formed by spinning after a water-soluble polymer is dissolved in water. The fibers in the nanofiber swelling layer are composed of water-based polyurethane and water-soluble polymer, have the function of self-closed pores, and are a good moisturizing material. The curing membrane has the characteristics of convenient laying, simple construction, thin thickness, and light weight. At the same time, the curing membrane has a small pore size and strong water retention capacity, and can achieve the purpose of long-term moisturizing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building construction, and in particular to a self-closed-cell moisturizing curing membrane and a preparation method thereof and application thereof in concrete curing. Background Art

[0002] The solidification process of cement concrete requires hydration reaction, which is inseparable from the participation of water. However, the poured concrete is affected by the external environment, and the water is easy to evaporate, resulting in a lack of water participation in the hydration reaction, resulting in incomplete solidification. Concrete that has not been cured is prone to cracks, honeycomb surface, sand loss and other phenomena.

[0003] There are two main methods of traditional maintenance. One is the covering maintenance method, in which a layer of covering material is covered on the surface of the poured concrete to reduce water evaporation and ensure the smooth progress of the concrete hydration reaction; the other is active water replenishment, which is continuous water replenishment by sprinkling or spraying. Covering maintenance often uses hemp (straw) bags, geotextiles, plastic films, etc. to cover the concrete surface. Among them, hemp (straw) bags and geotextiles are easily affected by dry air, especially in summer, when water evaporates quickly and the protective effect is poor. At the same time, hemp (straw) bags and geotextiles also have the disadvantages of being easy to rot and having a short life. Plastic films are easy to break and are generally used once. After being broken, plastic films pollute the environment. At the same time, there is also the problem that the film is easily blown up and folded by the wind, further exacerbating water loss and destroying the appearance of the concrete surface. Using spraying or sprinkling to maintain concrete can significantly improve the early strength of concrete, but it requires personnel to water and sprinkle water periodically, which is inefficient.

[0004] CN 113684743 A discloses a self-moisturizing concrete curing membrane and its preparation and laying method, which comprises a water-permeable non-woven fabric in the inner layer, a high molecular water-absorbing resin in the middle core layer and a water-blocking film in the surface layer, which are compounded by a binder to form a curing membrane. CN 206855716U discloses a concrete water-saving and moisturizing curing membrane, which comprises a water-impermeable membrane, a non-woven fabric, a water-absorbing membrane and a glue layer stacked in sequence.

[0005] Both of the above patent disclosures use water-absorbing particles as water storage materials. In order to increase the water storage capacity, a large amount is generally used. The powder particles are difficult to fix, and there are also problems such as hygroscopic expansion, which leads to a large thickness of the curing film. In addition, during the laying process, the moisturizing curing film needs to be made on-site and cannot be prefabricated, which makes the laying and removal processes complicated and has many limitations during use. Summary of the invention

[0006] In view of the technical problems that the moisturizing layer of the existing moisturizing curing membrane uses water-absorbing particles, resulting in a large thickness, a complicated laying process and an inability to replenish water again, the present invention provides a self-closed-pore moisturizing curing membrane and a preparation method thereof and an application in concrete curing. The membrane has the characteristics of thin thickness and easy laying. When used for concrete curing, the membrane can not only reduce water volatilization, but also replenish water in time through the membrane.

[0007] The technical solution of the present invention is a self-closed-pore moisturizing and curing film, comprising a moisturizing layer, a nanofiber hydrophobic layer, a nanofiber swelling layer and a protective layer arranged in sequence from bottom to top; the nanofiber hydrophobic layer is prepared from a hydrophobic polymer by an electrospinning process, and the nanofiber swelling layer is prepared from a water-soluble polymer by an electrospinning process.

[0008] Furthermore, the moisturizing layer is a hydrophilic non-woven fabric, and the protective layer is a water-permeable non-woven fabric; the surface density of the moisturizing layer and the protective layer are both 20-200g / m 2 ; The pore size of the protective layer is 0.1-0.2mm.

[0009] Furthermore, the thickness of the nanofiber hydrophobic layer and the nanofiber swelling layer is 0.1-0.5 mm respectively, the fiber diameter in the nanofiber hydrophobic layer and the nanofiber swelling layer is 0.3-3 μm, and the pore size is 0.5-2.5 μm.

[0010] The present invention also relates to a method for preparing the self-occluded pore moisturizing curing film, comprising the following steps:

[0011] S1, dissolving a hydrophobic polymer in a solvent to prepare a hydrophobic spinning solution, adding hydrophobic nanoparticles into the hydrophobic spinning solution, and then spraying a nanofiber hydrophobic layer on the moisturizing layer using an electrospinning technique;

[0012] S2, dissolving a water-soluble polymer in water to prepare a hydrophilic spinning solution, and then spraying a nanofiber swelling layer on the hydrophobic layer of the nanofiber obtained in S1 by using an electrospinning technique;

[0013] S3, covering the nanofiber swelling layer obtained in S2 with a protective layer, and subjecting the layer to ultrasonic compounding;

[0014] A self-closed-pore moisturizing curing film is obtained.

[0015] Furthermore, the hydrophobic polymer described in S1 is any one or more of polyurethane, polyacrylonitrile, polystyrene, polysulfone or polyvinylidene fluoride; the solvent is one or more of dichloromethane, chloroform, tetrahydrofuran, acetone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide; the hydrophobic nanoparticles are any one of silica, titanium oxide, aluminum oxide or montmorillonite.

[0016] Furthermore, the concentration of the hydrophobic polymer in the S1 hydrophobic spinning solution is 6-20 wt %, and the concentration of the hydrophobic nanoparticles is 0.1-0.5 wt %.

[0017] Furthermore, the water-soluble polymer in S2 is one or more of polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone or water-based polyurethane.

[0018] Furthermore, the water-soluble polymer is a mixture of polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone in a mass ratio of 1-5:1-7:1-8, wherein the molecular weight of polyethylene oxide is 200,000-2 million, the molecular weight of polyvinyl alcohol is 10,000-20,000, and the molecular weight of polyvinyl pyrrolidone is 500,000-2 million; the concentration of the water-soluble polymer in the hydrophilic spinning solution is 3-12wt%.

[0019] Furthermore, the process parameters of the electrospinning technology in S1 and S2 are: spinning voltage 10-30 kV, spinning solution flow rate 0.5-3.0 mL / h.

[0020] The present invention also relates to the application of the self-closed pore moisturizing curing membrane in concrete curing. During curing, water is first evenly sprayed on the moisturizing layer of the self-closed pore moisturizing curing membrane until it is saturated, and then covered on the concrete surface for curing; after curing for 5-15 days, water is evenly sprayed on the self-closed pore moisturizing curing membrane.

[0021] The present invention has the following beneficial effects:

[0022] 1. The curing film is provided with a nanofiber swelling layer and a nanofiber hydrophobic layer. The nanofiber hydrophobic layer is located above the moisturizing layer. Due to its hydrophobic property and void structure, it can prevent liquid water from penetrating outward as much as possible. Only a small amount of water vapor passes through the nanofiber hydrophobic layer and is absorbed by the nanofiber swelling layer. The water-soluble polymer of the nanofiber swelling layer will swell or dissolve to form a colloidal solution after meeting water. The colloidal solution will block the pores in the nanofiber hydrophobic layer, reduce the pore size and porosity, and even achieve closed pores, further reducing the evaporation of water.

[0023] 2. The present invention provides a moisturizing layer in the curing film, which is located between the nanofiber hydrophobic layer and the concrete, and can play a good role in water storage and retention. In addition, it cooperates with the nanofiber hydrophobic layer to isolate the nanofiber swelling layer from the concrete surface, and prevents the nanofiber swelling layer from being soaked in water too early. A protective layer is also provided above the nanofiber swelling layer to improve the strength of the curing film. In the process of spraying water in the later stage, the direct impact of the water flow on the nanofiber swelling layer and the concrete below it can be reduced. The pores on the protective layer are also conducive to the water infiltration into the concrete during the later water replenishment.

[0024] 3. The present invention can control the solubility by regulating the molecular weight of the water-soluble polymer in the nanofiber swelling layer, and can achieve different porosities of the nanofiber swelling layer at different curing stages by regulating the degree of fiber dissolution / swelling in the nanofiber swelling layer.

[0025] 4. If the concrete lacks water within a certain maintenance period, secondary water replenishment can be carried out. After spraying, the water penetrates into the nanofiber swelling layer, nanofiber hydrophobic layer and moisturizing layer through the protective layer in turn, and finally flows into the concrete to achieve secondary water replenishment; at the same time, when the nanofiber swelling layer comes into contact with water, part of the water-soluble material dissolves, and when the surface water evaporates, it causes adhesion and closed pores between the fibers, forming a waterproof film layer above the moisturizing layer, thus achieving long-term moisturizing again.

[0026] 5. The present invention reduces the volatilization of water and can perform secondary water replenishment, thereby avoiding the use of a heavy hygroscopic layer composed of water-absorbing particles. The total thickness of the prepared curing film is 0.5-1.5mm and the surface density is: 100-300g / m 2 . BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a structural diagram of a self-closed-cell moisturizing curing film, in which: 1, protective layer; 2, nanofiber swelling layer; 3, nanofiber hydrophobic layer; 4, moisturizing layer.

[0028] Figure 2 This is the morphology of the hydrophobic layer of the nanofibers in Example 1.

[0029] Figure 3 This is the morphology of the nanofiber swelling layer before closure in Example 1.

[0030] Figure 4 This is the morphology of the nanofiber swelling layer after pore closing in Example 1.

[0031] Figure 5 are the compressive strength and flexural strength of the mortar under different curing conditions in the test example.

[0032] Figure 6 is the compressive strength of concrete under different curing conditions in the test case.

[0033] Figure 7 This is the frost resistance of concrete under different curing conditions in the test example.

[0034] Figure 8 is the carbonation depth of concrete under different curing conditions in the test case.

[0035] Fig. 9 This is the internal pore image of concrete under covering curing conditions in the test case.

[0036] Fig.10 This is the internal pore image of concrete under standard curing conditions in the test case. DETAILED DESCRIPTION

[0037] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0038] Example 1

[0039] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0040] Preparation of the hydrophobic layer of nanofibers: polyurethane powder was dissolved in DMF, heated and stirred at 70°C for 8 hours to prepare a polyurethane spinning solution with a concentration of 12wt%, and then hydrophobic silica with a particle size of 100-150nm was added to the polyurethane spinning solution, stirred for 2 hours, and ultrasonically dispersed for 5 minutes, wherein the concentration of hydrophobic silica in the polyurethane spinning solution was 0.5wt%. Finally, the prepared polyurethane spinning solution was placed in an electrospinning machine for electrospinning, and the receiving substrate was a moisturizing layer with a surface density of 150g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 25kv, spinning solution flow rate 0.8mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 1h.

[0041] Preparation of nanofiber swelling layer: Dissolve waterborne polyurethane, polyethylene oxide and polyvinyl pyrrolidone in water at a mass ratio of 5:3:2, heat and stir at 60°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 4wt%. The molecular weight of polyethylene oxide is 1.3 million, and the molecular weight of polyvinyl pyrrolidone is 2 million. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning. The receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 20kv, spinning solution flow rate 1.5mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 1h.

[0042] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 80g / m 2 The pore size is 0.15mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0043] Example 2

[0044] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0045] Preparation of hydrophobic layer of nanofibers: Dissolve polystyrene (PS) slices in DMF, stir at room temperature for 8 hours to prepare a PS spinning solution with a concentration of 20wt%, then add hydrophobic silica with a particle size of 150-200nm to the PS spinning solution, continue stirring for 2 hours, and use ultrasonic dispersion for 5 minutes, wherein the concentration of hydrophobic silica in the PS spinning solution is 0.5wt%. Finally, place the prepared PS spinning solution in an electrospinning machine for electrospinning, and the receiving substrate adopts a surface density of 150g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 30kv, spinning solution flow rate 1.5mL / h, spinning needle head 20cm away from the receiving substrate, and spinning time 30min.

[0046] Preparation of nanofiber swelling layer: Dissolve polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone in water at a mass ratio of 1:1:1, heat and stir at 70°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 6wt%. The molecular weight of the polyethylene oxide is 1 million, the molecular weight of the polyvinyl alcohol is 20,000, and the molecular weight of the polyvinyl pyrrolidone is 500,000. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning, and the receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 25kv, spinning solution flow rate 1mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 1h.

[0047] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer, and the surface density of the polyester nonwoven fabric is 80g / m 2 The pore size is 0.15mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0048] Example 3

[0049] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0050] Preparation of the hydrophobic layer of nanofibers: Dissolve polyacrylonitrile powder in DMSO, heat and stir at 80°C for 12 hours to prepare a polyurethane spinning solution with a concentration of 6wt%, then add titanium oxide with a particle size of 100-150nm to the polyurethane spinning solution, continue stirring for 2 hours, and use ultrasonic dispersion for 5 minutes, wherein the concentration of titanium oxide in the polyurethane spinning solution is 0.1wt%. Finally, place the prepared polyurethane spinning solution in electrospinning for electrospinning, and the receiving substrate is the moisturizing layer, and the surface density is 200g / m 2The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 20kv, spinning solution flow rate 0.5mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 2h.

[0051] Preparation of nanofiber swelling layer: Mix and dissolve polyvinyl pyrrolidone with a molecular weight of 2 million in water, heat and stir at 70°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 3wt%. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning, and the receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 10kv, spinning solution flow rate 1mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 2h.

[0052] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer, and the surface density of the polyester nonwoven fabric is 20g / m 2 The pore size is 0.2mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0053] Example 4

[0054] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0055] Preparation of hydrophobic layer of nanofibers: Dissolve polyvinylidene fluoride powder in a mixed solution of DMF and acetone with a mass ratio of 7:3, heat and stir at 60℃ for 8 hours to prepare a polyvinylidene fluoride spinning solution with a concentration of 12wt%, then add montmorillonite with a particle size to the polyurethane spinning solution, continue stirring for 2 hours, and use ultrasonic dispersion for 5 minutes, where the concentration of montmorillonite in the polyvinylidene fluoride spinning solution is 0.3wt%. Finally, place the prepared polyurethane spinning solution in electrospinning for electrospinning, and the receiving substrate is a moisturizing layer with a surface density of 100g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 10kv, spinning solution flow rate 0.8mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 1h.

[0056] Preparation of nanofiber swelling layer: Dissolve water-based polyurethane and polyethylene oxide in water at a mass ratio of 1:1, heat and stir at 80°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 4wt%. The molecular weight of polyethylene oxide is 2 million. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning. The receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 15kv, spinning solution flow rate 1.5mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 2h.

[0057] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 100g / m 2 The pore size is 0.1mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0058] Example 5

[0059] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0060] Preparation of hydrophobic layer of nanofiber: Dissolve polysulfone particles in DMF, heat and stir at 80℃ for 10 hours to prepare polysulfone spinning solution with a concentration of 20wt%, then add alumina with a particle size of 100-150nm to the polysulfone spinning solution, continue stirring for 2 hours, and use ultrasonic dispersion for 5 minutes, wherein the concentration of hydrophobic silica in the polyurethane spinning solution is 0.3wt%. Finally, place the prepared polyurethane spinning solution in electrospinning for electrospinning, and the receiving substrate is the moisturizing layer, and the surface density is 200g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 15kv, spinning solution flow rate 1.2mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 1.5h.

[0061] Preparation of nanofiber swelling layer: Dissolve polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone in a mass ratio of 5:7:8 in water, heat and stir at 60°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 8wt%. The molecular weight of the polyethylene oxide is 200,000, the molecular weight of the polyvinyl alcohol is 10,000, and the molecular weight of the polyvinyl pyrrolidone is 1.5 million. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning, and the receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 20kv, spinning solution flow rate 1mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 1h.

[0062] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 50g / m 2 The pore size is 0.13mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0063] Example 6

[0064] A self-occluded pore moisturizing curing film, the preparation method of the curing film comprises the following steps:

[0065] Preparation of hydrophobic layer of nanofiber: Dissolve polyacrylonitrile and polyvinylidene fluoride powder in DMF with a mass ratio of 1:1, heat and stir at 80℃ for 10 hours to prepare a composite spinning solution with a concentration of 20wt%, then add alumina with a particle size of 100-150nm to the composite spinning solution, continue stirring for 2 hours, and use ultrasonic dispersion for 5 minutes, wherein the concentration of hydrophobic silica in the composite spinning solution is 0.1wt%. Finally, place the prepared polyurethane spinning solution in electrospinning for electrospinning, and the receiving substrate is the moisturizing layer, and the surface density is 200g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 15kv, spinning solution flow rate 1mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 1.5h.

[0066] Preparation of nanofiber swelling layer: Dissolve polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone in a mass ratio of 3:5:7 in water, heat and stir at 60°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 12wt%. The molecular weight of the polyethylene oxide is 800,000, the molecular weight of the polyvinyl alcohol is 15,000, and the molecular weight of the polyvinyl pyrrolidone is 500,000. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning, and the receiving substrate is a needle-punched cotton hygroscopic non-woven fabric sprayed with a nanofiber hydrophobic layer, and the nanofiber swelling layer is sprayed on the nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 20kv, spinning solution flow rate 1mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 1h.

[0067] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 60g / m 2 The pore size is 0.13mm. Finally, ultrasonic composite processing is performed to obtain a self-closed pore moisturizing curing film.

[0068] Comparative Example 1

[0069] A curing film, a method for preparing the curing film comprises the following steps:

[0070] Preparation of the hydrophobic layer of nanofibers: polyurethane powder was dissolved in DMF, heated and stirred at 70°C for 8 hours to prepare a polyurethane spinning solution with a concentration of 12wt%, and then hydrophobic silica with a particle size of 100-150nm was added to the polyurethane spinning solution, stirred for 2 hours, and ultrasonically dispersed for 5 minutes, wherein the concentration of hydrophobic silica in the polyurethane spinning solution was 0.5wt%. Finally, the prepared polyurethane spinning solution was placed in an electrospinning machine for electrospinning, and the receiving substrate was a moisturizing layer with a surface density of 150g / m 2 The needle-punched cotton hygroscopic nonwoven fabric is sprayed on it to obtain a nanofiber hydrophobic layer. The process parameters of electrospinning are: spinning voltage 25kv, spinning solution flow rate 0.8mL / h, spinning needle head 15cm away from the receiving substrate, and spinning time 1h.

[0071] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 80g / m 2 The pore size is 0.15mm. Finally, ultrasonic composite processing is performed to obtain a curing film.

[0072] Comparative Example 2

[0073] A curing film, a method for preparing the curing film comprises the following steps:

[0074] Preparation of nanofiber swelling layer: Dissolve waterborne polyurethane, polyethylene oxide and polyvinyl pyrrolidone in water at a mass ratio of 5:3:2, heat and stir at 60°C for 12 hours to prepare a hydrophilic spinning solution with a concentration of 4wt%. The molecular weight of polyethylene oxide is 1.3 million, and the molecular weight of polyvinyl pyrrolidone is 2 million. The prepared hydrophilic spinning solution is placed in electrospinning for electrospinning. The receiving substrate is a moisturizing layer with a surface density of 150g / m 2 Needle-punched cotton hygroscopic nonwoven fabric. The process parameters of electrospinning are: spinning voltage 20kv, spinning liquid flow rate 1.5mL / h, spinning needle head 15cm away from the receiving substrate, spinning time 1h.

[0075] A layer of polyester nonwoven fabric is covered on the nanofiber swelling layer as a protective layer. The surface density of the polyester nonwoven fabric is 80g / m 2 The pore size is 0.15mm. Finally, ultrasonic composite processing is performed to obtain a curing film.

[0076] The samples prepared in Examples 1-6 and Comparative Examples 1-2 were characterized in structure, and the average pore size of the nanofibers was measured using a fully automatic BET specific surface (area) analysis tester. Microscopic images of the nanofibers were randomly taken using a scanning electron microscope, and then the diameters of 100 fibers were randomly measured to obtain the average value as the diameter of the fiber. The thickness was measured using a fabric thickness gauge. The test results are shown in Table 1.

[0077] Table 1

[0078]

[0079]

[0080] Application Examples

[0081] The application of self-closed pore moisturizing curing membrane in concrete curing. During the specific curing, first clean the concrete surface to be cured, and evenly spray water on the moisturizing layer of the self-closed pore moisturizing curing membrane until saturation, and then cover the concrete surface for curing, with the moisturizing layer close to the concrete surface; after 10 days of curing, there is no need to lift the curing membrane, and directly spray water evenly on the protective layer of the self-closed pore moisturizing curing membrane to make the curing membrane completely soaked.

[0082] Test Case

[0083] The structure of the self-occluded pore moisturizing curing film obtained in Example 1 is as follows Figure 1 As shown, the morphology of the hydrophobic layer of the nanofiber is shown in Figure 2 , it can be seen that the fiber morphology is uniform; the morphology of the nanofiber swelling layer before closing the hole is shown in Figure 3 After being immersed in water at room temperature for 1 hour, the closed-pore morphology of the nanofiber swelling layer is shown in Figure 4 The fibers dissolve, the fibers adhere to each other, the gaps become smaller or even closed, and the air is isolated.

[0084] After the concrete is formed, it is covered with a moisture-retaining curing film and watered for curing, and the relevant properties after curing are measured. Before demolding, the concrete test blocks and mortar test blocks are respectively cured indoors and covered with the film as prepared in Example 1, and are uniformly placed in a standard curing room after demolding.

[0085] After the mortar specimens are formed, they are cured in different curing methods (24±2h) and then demoulded. They are then uniformly cured to the corresponding age and then taken out to measure the compressive strength and flexural strength. The test is based on the "Test Method for Strength of Cement Mortar" (GB / T17671-1999). The test results are as follows: Figure 5 and Figure 6 shown.

[0086] After the concrete specimens are formed, they are cured in different curing methods (24±2h) and then demolded. The specimens are then placed in a uniform environment and cured until the age, and then taken out to measure the compressive strength. The test is based on the "Standard for Test Methods for Physical and Mechanical Properties of Concrete" (GB / T50081-2019). The test results are as follows Figure 6 shown.

[0087] After the concrete specimens are formed, they are cured in different curing methods (24±2h) and then demolded. The specimens are then placed in a uniform environment and cured until the age, and then taken out to measure the frost resistance. The test is based on the "Test Procedure for Hydraulic Concrete" (SL / T 352-2020). The test results are as follows Figure 7 shown.

[0088] After the concrete specimens are formed, they are cured by different curing methods (24±2h) and then demolded. Then the specimens are placed in a uniform environment and cured until the age, then taken out and placed in a carbonation box. After carbonization to the age, the carbonation depth is tested. The carbon dioxide concentration in the carbonation box is 20%, the temperature is 20±3℃, and the relative humidity is 70%. The test is based on the "Test Procedures for Hydraulic Concrete" (SL / T 352-2020). The test results are as follows Figure 8 shown.

[0089] After the concrete specimen is formed, the bubble parameter analyzer is used to observe the pores inside the concrete. Figure 9-10 The sample in Example 1 was subjected to film curing, and compared with standard curing, the number and size of bubbles in the formed specimen were significantly reduced.

Claims

1. A self-occluded pore moisturizing and curing film, It is characterized in that The invention comprises a moisturizing layer, a nanofiber hydrophobic layer, a nanofiber swelling layer and a protective layer arranged in sequence from bottom to top; the nanofiber hydrophobic layer is prepared by an electrostatic spinning process of a hydrophobic polymer, and the nanofiber swelling layer is prepared by an electrostatic spinning process of a water-soluble polymer; the moisturizing layer is a hydrophilic non-woven fabric, and the protective layer is a water-permeable non-woven fabric; the surface density of the moisturizing layer and the protective layer are both 20-200g / m 2 The pore size of the protective layer is 0.1-0.2 mm; the thickness of the nanofiber hydrophobic layer and the nanofiber swelling layer are 0.1-0.5 mm respectively, the fiber diameter in the nanofiber hydrophobic layer and the nanofiber swelling layer is 0.3-3 μm, and the pore size is 0.5-2.5 μm.

2. A method for preparing the self-occluded pore moisturizing curing film according to claim 1, It is characterized in that The following steps are involved: S1, dissolving a hydrophobic polymer in a solvent to prepare a hydrophobic spinning solution, adding hydrophobic nanoparticles into the hydrophobic spinning solution, and then spraying a nanofiber hydrophobic layer on the moisturizing layer using an electrospinning technique; S2, dissolving a water-soluble polymer in water to prepare a hydrophilic spinning solution, and then spraying a nanofiber swelling layer on the hydrophobic layer of the nanofiber obtained in S1 by using an electrospinning technique; S3, covering the nanofiber swelling layer obtained in S2 with a protective layer, and subjecting the layer to ultrasonic compounding; A self-closed-pore moisturizing curing film is obtained.

3. The method for preparing the self-occluded pore moisturizing curing film according to claim 2, It is characterized in that The hydrophobic polymer described in S1 is any one or more of polyurethane, polyacrylonitrile, polystyrene, polysulfone or polyvinylidene fluoride; the solvent is one or more of dichloromethane, chloroform, tetrahydrofuran, acetone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide; the hydrophobic nanoparticles are any one of silica, titanium oxide, aluminum oxide or montmorillonite.

4. The method for preparing the self-occluded pore moisturizing curing film according to claim 2, It is characterized in that The concentration of the hydrophobic polymer in the S1 hydrophobic spinning solution is 6-20wt%, and the concentration of the hydrophobic nanoparticles is 0.1-0.5wt%.

5. The method for preparing the self-occluded pore moisturizing curing film according to claim 2, Features: The water-soluble polymer in S2 is one or more of polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone or water-based polyurethane.

6. The method for preparing the self-occluded pore moisturizing curing film according to claim 5, It is characterized in that The water-soluble polymer is a mixture of polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone in a mass ratio of 1-5:1-7:1-8, wherein the molecular weight of polyethylene oxide is 200,000-2 million, the molecular weight of polyvinyl alcohol is 10,000-20,000, and the molecular weight of polyvinyl pyrrolidone is 500,000-2 million; the concentration of the water-soluble polymer in the hydrophilic spinning solution is 3-12wt%.

7. The method for preparing the self-occluded pore moisturizing curing film according to claim 2, Features: The process parameters of the electrospinning technology in S1 and S2 are: spinning voltage 10-30 kV, spinning solution flow rate 0.5-3.0 mL / h.

8. Application of the self-closed-cell moisturizing curing membrane according to claim 1 in concrete curing, Features: During specific maintenance, first spray water evenly on the moisturizing layer of the self-closed pore moisturizing curing membrane until it is saturated, and then cover it on the concrete surface for maintenance; after 5-15 days of maintenance, spray water evenly on the self-closed pore moisturizing curing membrane.