Semiconductor material loaded noble metal oxide catalyst and preparation method and application thereof
By using semiconductor materials to support precious metal oxide catalysts in proton exchange membrane water electrolysis technology, the problems of slow anodizing reaction kinetics and scarce and expensive precious metal ruthenium catalysts are solved, achieving efficient and stable acidic water oxidation catalysis and reducing OER. overpotential and reduce costs.
Patent Information
- Application Number
- CN202211673418.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-26
AI Technical Summary
In the existing proton exchange membrane water electrolysis technology, the anodic oxidation reaction (OER) suffers from slow reaction kinetics and poor stability in acidic environments, and the precious metal ruthenium (Ru) catalyst is scarce and expensive, which limits its large-scale application.
Semiconductor materials are used to support precious metal oxide catalysts. Through room temperature hydrothermal reaction and subsequent temperature-raising treatment, RuO2/VO-WO3 catalysts with high activity and stability are prepared, and particle-carrier interactions are used to improve catalytic performance.
It effectively reduces the overpotential of OER, increases the mass activity of the catalyst, shows excellent catalytic performance and stability, has low cost, and is suitable for large-scale development and utilization.
Smart Images

Figure HDA0004017056540000011 
Figure HDA0004017056540000012 
Figure HDA0004017056540000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy material technology and electrochemical catalysis technology, and specifically relates to a semiconductor material-loaded noble metal oxide catalyst and a preparation method and application thereof. Background Art
[0002] Proton exchange membrane water electrolysis (PEMWEs) is widely regarded as an ideal technology for storing intermittent solar or wind energy as sustainable hydrogen due to its high energy efficiency, high yield and purity. Water electrolysis consists of two half reactions: the cathode hydrogen evolution reaction (HER) and the anode oxygen evolution reaction (OER). Compared with the lower energy loss of the cathode HER, the anode OER still has the problems of slow reaction kinetics and poor stability in acidic environment, which has become the main bottleneck for the practical application of PEMWEs. Therefore, the development of efficient and cheap OER catalysts under acidic conditions is the most difficult and challenging of all water electrolysis technologies. At present, the catalysts of PEMWE anode are mainly based on precious metal ruthenium (Ru)-based metals and their oxides. However, their scarcity and high price are the main obstacles to their large-scale application. In order to fully utilize the advantages of PEMWEs and balance the relationship between price and catalytic activity, it is imperative to develop highly active and stable OER catalysts with low Ru content. Summary of the invention
[0003] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art, and proposes a semiconductor material-loaded precious metal oxide catalyst and its preparation method and application. The semiconductor oxide-loaded precious metal oxide as an acidic water oxidation catalyst effectively reduces the overpotential of OER, gives full play to the synergistic effect of the interaction between particles and carriers on the particles and carriers, and exhibits excellent catalytic performance in the application of acidic water oxidation.
[0004] The technical solution of the present invention is:
[0005] A method for preparing a semiconductor material-supported noble metal oxide catalyst comprises the following steps:
[0006] (1) At room temperature, chlorate containing W metal ions is added to a quantitative ethanol solution and stirred to dissolve all the metal salts, then an ethanol solution containing RuCl3 is added and stirred until the mixture is uniformly mixed, and then the obtained mixed solution is transferred to a reactor for hydrothermal reaction, and the mixture is naturally cooled to room temperature after the reaction is complete;
[0007] The purpose of stirring the two solutions until they are uniformly mixed is to allow the W ions and Ru ions to be fully mixed in the solvent so that they can form a semiconductor material loaded with a noble metal oxide material during the hydrothermal process;
[0008] (2) centrifuging the product obtained in step (1), washing it multiple times, and then transferring it to a vacuum box until it is completely dried;
[0009] The purpose of centrifugation and washing is to wash away inactive substances present in the catalyst;
[0010] (3) The solid obtained in step (2) is transferred to a porcelain boat in a tube furnace, and the temperature is increased to 300-400° C. at a constant heating rate in an air atmosphere, and the constant temperature is maintained for 1.5 h to 2.5 h, and finally cooled to room temperature to obtain a semiconductor material loaded with precious metal oxides.
[0011] Furthermore, in the step (1), 20-25 mg of chlorate of W metal ion is dissolved in 10-15 mL of ethanol, and the molar ratio of the added RuCl3 to the chlorate of W metal ion is 1:2. The volume of ethanol for dissolving RuCl3 is in the range of 1-5 mL, and the volume of ethanol is mainly sufficient to completely dissolve RuCl3.
[0012] Furthermore, the chlorate containing W metal ions in step (1) is tungsten hexachloride.
[0013] Furthermore, in step (1), the stirring time for dissolving the metal salt is 20 to 30 minutes, and the stirring time for the mixed solution is 10 to 20 minutes.
[0014] Furthermore, the hydrothermal reaction temperature in step (1) is 180-210° C., and the reaction time is 8-12 hours.
[0015] Furthermore, the centrifugal treatment time in step (2) is 3 to 5 minutes, and the centrifugal speed is 8000 to 12000 r / min.
[0016] Furthermore, the vacuum drying time in step (2) is 8 to 12 hours.
[0017] Furthermore, the heating rate in step (3) is 3-5°C / min.
[0018] The present invention also protects the semiconductor material loaded noble metal oxide catalyst prepared by the preparation method.
[0019] The present invention also protects the use of the semiconductor material-supported noble metal oxide catalyst prepared by the preparation method in acidic water oxidation.
[0020] Beneficial effects of the present invention:
[0021] The present invention aims to solve the problems of expensive and limited resources of acidic water oxidation catalysts in the prior art, and provides a semiconductor oxide-supported noble metal oxide catalyst, which has high conductivity and specific surface area, and effectively reduces the overpotential of OER, and is a relatively ideal OER reaction process. Compared with the prior art, the semiconductor oxide-supported noble metal oxide catalyst provided by the present invention is applied to acidic water oxidation and has the following advantages:
[0022] (1) The catalyst prepared by the present invention was applied to acidic water oxidation, and the mass activities at overpotentials of 300 mV (1.53 V vs. RHE) and 370 mV (1.6 V vs. RHE) were 27110 A g -1 Ru and 55977A g -1 Ru , which are 10.8 and 10.9 times of commercial RuO2 respectively;
[0023] (2) The semiconductor oxide loaded with noble metal oxide prepared by the present invention has excellent OER activity, and in the stability test, the catalyst exhibits excellent stability performance;
[0024] (3) The catalyst prepared by the present invention is a non-precious metal-supported precious metal oxide catalyst, which has a simple preparation process, readily available raw materials, low cost, and is conducive to large-scale development and utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the XRD pattern of RuO2 / VO-WO3 prepared in Example 1;
[0026] Figure 2 This is the SEM image of RuO2 / VO-WO3 prepared in Example 1;
[0027] Figure 3 TEM image of RuO2 / VO-WO3 prepared in Example 1;
[0028] Figure 4 The performance test results of the catalysts in Example 1 and Comparative Example 1 are shown in FIG. Figure 4 a is the LSV comparison chart, b is the Tafel slope comparison chart, and c is the stability comparison chart;
[0029] Figure 5 The results are a comparison of the mass activities of the catalysts of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] In order to further understand the present invention, the present invention will be further described in conjunction with the accompanying drawings and embodiments.
[0032] The present invention provides a method for preparing a semiconductor material-supported noble metal oxide catalyst for acidic water oxidation, comprising the following steps:
[0033] (1) At room temperature, add 20-25 mg of WCl6 into 10-15 mL of ethanol solution and stir vigorously for 20-30 min to dissolve all the metal salts. The metal salt solution obtained after dissolution is a transparent light yellow solution;
[0034] (2) according to the molar ratio of RuCl3 to WCl6 of 1:2, 5-7 mg of RuCl3 is dissolved in 1-5 mL of ethanol solution, the RuCl3 solution obtained in step (2) is added to (1), the two are stirred for 10-20 min until they are uniformly mixed, and then the solution is transferred to a reactor for hydrothermal reaction. The hydrothermal reaction temperature is maintained at 180-210° C., the hydrothermal time is 8-12 h, and the temperature is naturally cooled to room temperature after the reaction is completed;
[0035] (3) centrifuging the material after cooling the reactor in step (2) for 3 to 5 minutes at a centrifugal speed of 10,000 r / min, washing multiple times, and then transferring to a vacuum box for 8 to 12 hours until completely dried;
[0036] (4) The solid obtained in step (3) is transferred to a porcelain boat in a tubular furnace, and the temperature is increased to 300°C to 400°C at a constant heating rate of 3 to 5°C / min in an air atmosphere, and the constant temperature is maintained for 1.5 to 2.5 hours, and finally cooled to room temperature to obtain a semiconductor material loaded with precious metal oxides.
[0037] Example 1
[0038] A method for preparing a semiconductor material-supported noble metal oxide catalyst for acidic water oxidation, comprising the following steps:
[0039] At room temperature, 20.588 mg WCl6 was dissolved in 14 mL ethanol, and stirred vigorously for 30 min to form a transparent light yellow solution. Then, 1 mL of 5.3845 mg RuCl3 ethanol solution was added, and stirred for 10 min until the two were mixed evenly. Then, the mixture was transferred to a reactor and hydrothermal heated at 200 ° C for 12 hours, and cooled naturally. The speed was set to 10000 r / min, centrifuged for 3 min, washed with anhydrous ethanol 3 times, and vacuum dried at 27 ° C for 10 h. Finally, the mixture was placed in a tube furnace and annealed at 400 ° C for 2 hours, with a calcination rate of 5 ° C / min. The product was named RuO2 / V O -WO3.
[0040] The RuO2 / V prepared above O -WO3 catalyst was characterized for material morphology. Figure 1 RuO2 / V O -XRD pattern of WO3 catalyst, such as Figure 2 RuO2 / V O -SEM image of WO3 catalyst, such as Figure 3 RuO2 / V O -TEM image of WO3 catalyst.
[0041] The final product RuO2 / V O -WO3 catalyst, electrochemical performance test using glassy carbon electrode and electrochemical workstation
[0042] Example 2
[0043] A method for preparing a semiconductor material-supported noble metal oxide catalyst for acidic water oxidation, comprising the following steps:
[0044] At room temperature, 22 mg of WCl6 was accurately weighed and dissolved in 12 mL of ethanol. The mixture was stirred vigorously for 20 min to form a transparent light yellow solution. Then, 3 mL of ethanol solution of 5.754 mg of RuCl3 was added and stirred for 15 min until the two were evenly mixed. The mixture was then transferred into a reactor and hydroheated at 180 ° C for 8 hours and cooled naturally. The speed was set to 10000 r / min, centrifuged for 4 min, washed with anhydrous ethanol for 3 times, and vacuum dried at 27 ° C for 8 h. Finally, the mixture was placed in a tubular furnace and annealed at 300 ° C for 1.5 hours with a calcination rate of 3 ° C / min to obtain the product.
[0045] Example 3
[0046] A method for preparing a semiconductor material-supported noble metal oxide catalyst for acidic water oxidation, comprising the following steps:
[0047] At room temperature, 25 mg WCl6 was accurately weighed and dissolved in 15 mL ethanol. The mixture was stirred vigorously for 25 min to form a transparent light yellow solution. Then, 5 mL of ethanol solution of 6.538 mg RuCl3 was added and stirred for 20 min until the two were evenly mixed. The mixture was then transferred into a reactor and hydroheated at 210 °C for 10 hours and cooled naturally. The speed was set to 10000 r / min, centrifuged for 5 min, washed with anhydrous ethanol for 3 times, and vacuum dried at 27 °C for 12 h. Finally, the mixture was placed in a tubular furnace and annealed at 350 °C for 2.5 hours with a calcination rate of 4 °C / min to obtain the product.
[0048] Comparative Example 1
[0049] Commercial RuO2 was used as the electrocatalyst. The OER electrocatalytic performance of the commercial RuO2 catalyst was measured on an electrochemical workstation.
[0050] Test Example 1
[0051] The final product obtained in Example 1 was used as a catalyst to perform an electrochemical performance test using a glassy carbon electrode and an electrochemical workstation. At the same time, the commercial RuO2 catalyst of Comparative Example 1 was also tested for performance, and the test results of the two were compared.
[0052] The performance of the catalyst prepared in Example 1 and the electrocatalyst prepared in Comparative Example 1 were tested and compared. Figure 4 The performance test comparison results shown in Figure 5 The mass activity comparison results are shown. Figure 4 It can be seen that the overpotential of RuO2 / VO-WO3 catalyst in acidic solution and the stability at the same current density have far exceeded the catalytic performance of commercial ruthenium dioxide catalyst.
[0053] pass Figure 4 and Figure 5 The performance test results show that the performance and stability of the catalyst prepared by the method of the present invention are better than those of commercial RuO2.
[0054] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a semiconductor material-supported noble metal oxide catalyst, characterized in that: The following steps are involved: (1) At room temperature, a chlorate containing W metal ions is added to a quantitative ethanol solution and stirred to dissolve all the metal salts, and then an ethanol solution containing RuCl3 is added, wherein the molar ratio of the added RuCl3 to the chlorate containing W metal ions is 1:2, and the mixture is stirred until the mixture is uniformly mixed, and then the obtained mixed solution is transferred to a reactor, and a hydrothermal reaction is carried out at 180-210° C. After the reaction is completed, the mixture is naturally cooled to room temperature; (2) centrifuging the product obtained in step (1), washing it multiple times, and then transferring it to a vacuum box until it is completely dried; (3) The solid obtained in step (2) is transferred to a porcelain boat in a tube furnace, and the temperature is increased to 300-400° C. at a constant heating rate in an air atmosphere, and the constant temperature is maintained for 1.5 h to 2.5 h, and finally cooled to room temperature to obtain a semiconductor material loaded with precious metal oxides.
2. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: In the step (1), 20-25 mg of chlorate of W metal ion is dissolved in 10-15 mL of ethanol.
3. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: The chlorate containing W metal ions in step (1) is tungsten hexachloride.
4. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: In the step (1), the stirring time for dissolving the metal salt is 20 to 30 minutes, and the stirring time for the mixed solution is 10 to 20 minutes.
5. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: The hydrothermal reaction temperature in step (1) is 180-210° C., and the reaction time is 8-12 hours.
6. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: The centrifugal treatment time in step (2) is 3 to 5 minutes, and the centrifugal speed is 8000 to 12000 r / min.
7. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: The vacuum drying time in step (2) is 8 to 12 hours.
8. The method for preparing a semiconductor material-supported noble metal oxide catalyst according to claim 1, characterized in that: The heating rate in step (3) is 3-5°C / min.
9. The semiconductor material-supported noble metal oxide catalyst obtained by the preparation method according to any one of claims 1 to 8.
10. Use of a semiconductor material-supported noble metal oxide catalyst prepared by the preparation method according to any one of claims 1 to 8 in acidic water oxidation.