A kind of anti-collision and anti-slip heat-activated protective glue and preparation method thereof
By using thermally activated protective adhesives prepared with specific component proportions and drying treatment in the photovoltaic module industry, the problem of cardboard shell corner protection cannot meet the insufficient automatic bonding and anti-slip rub performance, and efficient automated production and Anti-slip rub effect.
Patent Information
- Application Number
- CN202210923940.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-08-02
AI Technical Summary
In the existing photovoltaic module industry, cardboard case angle guards cannot meet the needs of automated fitting, and existing adhesives have shortcomings in anti-slip rub performance.
A thermally activated protective adhesive that is anti-collision-resistant and slip-resistant, and the preparation materials include ethyl acetate, xylene, polyurethane polymer, tackifying resin, filler and antioxidant. Through specific component ratios and drying treatment, the Heat-activated PET tape with high bond strength, heat resistance and anti-slip rub performance.
It achieves high bonding strength, peel strength and heat resistance, and through the action of polyurethane polymer with other components, the friction coefficient of the tape is enhanced, achieving excellent anti-slip rub and anti-collision effect, suitable for automated production, and improving Production efficiency in the photovoltaic module industry.
Smart Images

Figure CN115851205B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesives, and in particular to an anti-collision and anti-slip heat-activated protective adhesive and a preparation method thereof. Background Art
[0002] In the photovoltaic module industry, cardboard corner protectors are widely used to prevent back panels from slipping and rubbing. Cardboard corner protectors have the advantages of good anti-slip effect and low cost. However, with the development of the photovoltaic industry, the demand for automation to improve efficiency is getting higher and higher. Cardboard needs to be placed manually, which cannot meet the automation requirements.
[0003] Chinese patent application CN201811172069.7 discloses a one-component solvent-free polyurethane adhesive for photovoltaic module backplane composite and a preparation method. The polyurethane prepolymer with a solid content of 100% is prepared by high-temperature polymerization reaction using polyol and diisocyanate as raw materials, compounding catalyst, leveling agent, antioxidant, and light stabilizer. The adhesive has high initial bonding strength, resistance to moisture and heat aging, resistance to yellowing, and weather resistance, which is beneficial to improving the weathering and yellowing resistance of the photovoltaic module backplane. Chinese patent application CN201810998421.6 discloses a water-blocking tape for photovoltaic module frames and its preparation method and use, including wood resin, curing agent, antioxidant, ultraviolet absorber, wherein the mother resin is a silicone pressure-sensitive adhesive or a polyurethane pressure-sensitive adhesive, which has suitable softness, is bonded to the cracks of the aluminum frame and the photovoltaic glass, does not fall off or turn yellow after long-term outdoor use, and does not leave residual glue when torn, but its bonding strength is low, the initial adhesion is only 13.4-23.7N / 25mm, and it does not have certain anti-collision and anti-skid properties. The technical problem to be solved by the present invention is to provide a heat-activated PET tape that can meet the requirements of automatic bonding to prevent skids. Summary of the invention
[0004] In order to solve the above problems, the first aspect of the present invention provides an anti-collision and anti-slip heat-activated protective glue, and the raw materials for its preparation, calculated by mass percentage, include:
[0005] Ethyl acetate 25-35%, xylene 15-25%, polyurethane polymer 40-50%, tackifying resin 5-15%, filler 0.5-2%, antioxidant 0.1-1%.
[0006] In some preferred embodiments, the raw materials for preparing the polyurethane polymer include polyester polyol, polyether polyol, isocyanate, hydrophilic chain extender, and catalyst; preferably, the raw materials for preparing the polyurethane polymer include 50 to 63 parts by weight of polyester polyol, 27 to 38 parts by weight of polyether polyol, 12 to 24 parts by weight of isocyanate, 0.5 to 2 parts by weight of hydrophilic chain extender, and 0.2 to 1.5 parts by weight of catalyst.
[0007] In some preferred embodiments, the polyester polyol is selected from one or more of polyethylene adipate glycol ester diol, polyethylene adipate glycol butylene glycol ester diol, poly(1,4-butylene adipate glycol) ester diol, polyethylene adipate glycol diethylene glycol ester diol, polyethylene adipate glycol diethylene glycol ester diol, polyester polyol of phthalic acid / octylpentanediol condensation, polyester polyol of sebacic acid / isophthalic acid / hexanediol / neopentyl glycol, polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol, and polyester polyol of adipic acid / isophthalic acid / terephthalic acid / neopentyl glycol / ethylene glycol; preferably, the polyester polyol is polyethylene adipate glycol ester diol and polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol.
[0008] In some preferred embodiments, the weight ratio of the polyethylene adipate diol to the polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol is (1.2-2.3):1; preferably, the weight ratio of the polyethylene adipate diol to the polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol is 1.6:1.
[0009] In some preferred embodiments, the average molecular weight of the polyethylene adipate diol is 1000-4000, the viscosity at 75°C is 400-800cps, and the hydroxyl value is 25-100mgKOH / g. Preferably, the average molecular weight of the polyethylene adipate diol is 300, the viscosity at 75°C is 700cps, and the hydroxyl value is 35-39mgKOH / g.
[0010] In some preferred embodiments, the polyether polyol is selected from one or more of polypropylene oxide ether polyol, propylene oxide ethylene oxide copolyether polyol, polytetramethylene ether polyol, polytetramethylene ether glycol, silane-modified polyether polyol, and aliphatic polyether polyol; preferably, the polyether polyol is polypropylene oxide ether polyol and silane-modified polyether polyol.
[0011] In some preferred embodiments, the mass ratio of the polypropylene oxide ether polyol to the silane-modified polyether polyol is 1:(1-2); preferably, the mass ratio of the polypropylene oxide ether polyol to the silane-modified polyether polyol is 1:1.2.
[0012] In some preferred embodiments, the functionality of the polypropylene oxide ether polyol is 2-4, the viscosity range at 25°C is 200-400 mPa·s, and the hydroxyl value is 50-60 mgKOH / g; preferably, the functionality of the polypropylene oxide ether polyol is 2, the viscosity range at 25°C is 270-370 mPa·s, and the hydroxyl value is 54.5-57.5 mgKOH / g.
[0013] In some preferred embodiments, the functionality of the silane-modified polyether polyol is 0.1-2, and the viscosity at 25°C is 10000-30000 mPa·s; preferably, the functionality of the silane-modified polyether polyol is 0.14-0.21, and the viscosity at 25°C is 21000 mPa·s.
[0014] In the present application, the polyurethane adhesive formed by polyether polyol and polyester polyol under the action of isocyanate has good strength. When the polyether polyol is selected as polypropylene oxide ether polyol and silane-modified polyether polyol, the holding force of the tape can also be increased. It is speculated that the possible reason is that polypropylene oxide ether polyol is a non-clean polyether polyol, contains side methyl groups, and has an incomplete structure. Moreover, the end group of silane-modified polyether polyol can be cured to form an elastomer with Si-O-Si as the skeleton after hydrolysis. The two are used in combination to increase the formation of hydrogen bonds between soft segments and hard segments in polyurethane, and at the same time enhance the interaction between hard segments, which is conducive to the enhancement of bonding strength and holding force. The applicant unexpectedly found that when the mass ratio of polypropylene oxide ether polyol and silane-modified polyether polyol is 1: (1-2), the compatibility of the components in the system can be increased, thereby increasing the mechanical strength, softness, elasticity and aging resistance of the protective glue, and playing a good anti-skid role.
[0015] In some preferred embodiments, the isocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, p-toluenesulfonyl isocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate; preferably, the isocyanate is diphenylmethane diisocyanate and hexamethylene diisocyanate.
[0016] In some preferred embodiments, the mass ratio of diphenylmethane diisocyanate to hexamethylene diisocyanate is 1:(0.7-1.3); preferably, the mass ratio of diphenylmethane diisocyanate to hexamethylene diisocyanate is 1:1.
[0017] In some preferred embodiments, the hydrophilic chain extender is selected from one or more of N-methyldiethanolamine, N-butyldiethanolamine, dimethylolpropionic acid, sodium ethylenediamine ethanesulfonate, dimethylolpropionic acid (DMPA), dihydroxymethylbutyric acid (DMBA), tartaric acid, dimethylolbutyric acid, and dimethylolpropionic acid; preferably, the hydrophilic chain extender is N-butyldiethanolamine and dimethylolbutyric acid.
[0018] In some preferred embodiments, the mass ratio of N-butyl diethanolamine to dihydroxymethyl butyric acid is 1:(2.1-2.7); preferably, the mass ratio of N-butyl diethanolamine to dihydroxymethyl butyric acid is 1:2.3.
[0019] In some preferred embodiments, the catalyst is selected from one or more of triethylamine, triethylenediamine, dibutyltin dilaurate, stannous octoate, dibutyltin dichloride, dibutyltin diacetate, 1,3,5-tris(dimethylaminopropyl)hexahydrotriazine, 2,4,6-tris(dimethylaminomethyl)phenol, bismorpholine diethyl ether, and diazabicyclo; preferably, the catalyst is dibutyltin dilaurate.
[0020] In some preferred embodiments, the tackifying resin is one or more of epoxy resin, phenolic resin, acrylate resin, rosin resin, terpene phenolic resin, petroleum resin, phosphate resin, and hydrogenated resin; preferably, the tackifying resin is terpene phenolic resin.
[0021] In some preferred embodiments, the average molecular weight of the terpene phenolic resin is 600-800, the acid value is 40-70 mgKOH / g, and the softening point is 140-170°C; preferably, the average molecular weight of the terpene phenolic resin is 690, the acid value is 45-60 mgKOH / g, and the softening point is 145-160°C.
[0022] In some preferred embodiments, the filler is selected from one or more of titanium dioxide, calcium carbonate, carbon black, talc, mica powder, aluminum dioxide, silicon dioxide, barium sulfate, pumice powder, aluminum hydroxide, and diatomaceous earth; preferably, the filler is calcium carbonate.
[0023] In some preferred embodiments, the calcium carbonate is selected from one or more of heavy calcium carbonate and light calcium carbonate; preferably, the calcium carbonate is heavy calcium carbonate; further preferably, the average particle size of the heavy calcium carbonate is 700-1300 mesh; further preferably, the average particle size of the heavy calcium carbonate is 800 mesh.
[0024] In some preferred embodiments, the antioxidant is selected from one or more of 2,6-di-tert-butyl-cresol, pentaerythritol tetrakis(4-hydroxy-3,5-tert-butylphenylpropionate), 3.5-di-tert-butyl-4-hydroxyphenylpropionate octadecyl, triphenyl phosphite, and tris(nonylphenyl) phosphite; preferably, the antioxidant is 2,6-di-tert-butyl-cresol.
[0025] The second aspect of the present invention provides a method for preparing a collision-proof and anti-slip heat-activated protective adhesive, which comprises the following steps:
[0026] S1. After mixing the prepared raw materials, apply them once on the upper surface of the PET substrate;
[0027] S2. Dry the sample obtained in S1 through a drying oven.
[0028] In S2, the drying tunnel is a three-stage drying.
[0029] Preferably, the drying temperature of the first drying tunnel is 70-95°C, and the time is 0.5-3 min; the drying temperature of the second drying tunnel is 100-130°C, and the time is 1-5 min; the drying temperature of the third drying tunnel is 140-160°C, and the time is 2-5 min.
[0030] Further preferably, the drying temperature of the first drying tunnel is 80°C for 1 min; the drying temperature of the second drying tunnel is 120°C for 2.5 min; the drying temperature of the third drying tunnel is 150°C for 2.5 min.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The protective adhesive prepared by mixing ethyl acetate, xylene, polyurethane polymer, tackifying resin, filler and antioxidant in the present invention has excellent bonding strength and peeling strength after heating, which can reach 60N / 25mm. The heat-activated protective adhesive also exhibits excellent heat resistance and has certain softness and resilience. In addition, the specific polyurethane polymer can increase the friction coefficient of the protective adhesive by interacting with other components in the system, thereby achieving anti-slip and anti-collision effects.
[0033] (2) The protective adhesive obtained by the present invention is a heat-activated protective adhesive, which is attached to the aluminum frame of the component by an automatic tape sticking machine and then automatically pressed by a hot press. After pressing, it has a very high bonding strength and can play a role in preventing slipping and scratching.
[0034] (3) The heat-activated protective adhesive obtained by the present invention has good processability, can realize automated production, reduce labor, and improve production efficiency. It can be widely used in the photovoltaic module industry to achieve good anti-slip and anti-collision effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Example and comparative sample processing flow chart
[0036] Figure 2 Result diagram of displacement test of sample 1 at 80°C after pressing for 5s (left) and 10s (right) in the samples obtained in Example 1
[0037] Figure 3 Result diagram of displacement test of sample 2 at 80°C after pressing for 5s (left) and 10s (right) in the samples obtained in Example 1
[0038] Figure 4 The residual glue on the surface of the aluminum part after the peeling force test of the sample obtained in Example 1.
[0039] Figure 5 Peel force test result curve of the samples obtained in Example 1. DETAILED DESCRIPTION
[0040] Example 1
[0041] 1. A heat-activated protective adhesive for anti-collision and anti-slip properties, the raw materials for its preparation, calculated by mass percentage, include:
[0042] Ethyl acetate 30%, xylene 17%, polyurethane polymer 45%, tackifying resin 7%, filler 0.8%, antioxidant 0.2%.
[0043] The raw materials for preparing the polyurethane polymer include 55 parts by weight of polyester polyol, 32 parts by weight of polyether polyol, 18 parts by weight of isocyanate, 0.8 parts by weight of hydrophilic chain extender, and 0.4 parts by weight of catalyst.
[0044] The polyester polyol is polyethylene adipate glycol and a polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol.
[0045] The weight ratio of the polyethylene adipate diol to the polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol is 1.6:1.
[0046] The polyethylene adipate glycol has an average molecular weight of 300, a viscosity of 700 cps at 75° C., and a hydroxyl value of 35 to 39 mgKOH / g (Jining Tangyi Chemical Co., Ltd., HY-3020).
[0047] The CAS number of the polyester polyol of 1,6-hexanediol / 1.6-hexanediol / neopentyl glycol is 25214-14-6.
[0048] The polyether polyols are polypropylene oxide ether polyols and silane-modified polyether polyols.
[0049] The mass ratio of the polyoxypropylene ether polyol to the silane-modified polyether polyol is 1:1.2.
[0050] The functionality of the polyoxypropylene ether polyol is 2, the viscosity range at 25° C. is 270 to 370 mPa·s, and the hydroxyl value is 54.5 to 57.5 mgKOH / g (Green Union (Jining) Chemical Technology Co., Ltd., DL-2000D).
[0051] The functionality of the silane-modified polyether polyol is 0.14-0.21, and the viscosity at 25° C. is 21000 mPa·s (Dow, VORASIL 602).
[0052] The isocyanate is diphenylmethane diisocyanate and hexamethylene diisocyanate.
[0053] The mass ratio of the diphenylmethane diisocyanate to hexamethylene diisocyanate is 1:1.
[0054] The hydrophilic chain extender is N-butyl diethanolamine and dimethylol butyric acid.
[0055] The mass ratio of the N-butyl diethanolamine to dihydroxymethyl butyric acid is 1:2.3.
[0056] The catalyst is dibutyltin dilaurate.
[0057] The tackifying resin is terpene phenolic resin.
[0058] The terpene phenolic resin has an average molecular weight of 690, an acid value of 45-60 mgKOH / g, and a softening point of 145-160° C. (Shandong Guangshen Electronic Technology Co., Ltd., 803L).
[0059] The filler is calcium carbonate.
[0060] The calcium carbonate is heavy calcium carbonate; the average particle size of the heavy calcium carbonate is 800 meshes (Guangxi Zhe Chuang Chemical Co., Ltd.).
[0061] The antioxidant is 2,6-di-tert-butyl-cresol.
[0062] 2. A method for preparing a collision-proof and anti-slip heat-activated protective adhesive, comprising the following steps:
[0063] S1. After mixing the prepared raw materials, apply them once on the upper surface of the PET substrate;
[0064] S2. Dry the sample obtained in S1 through a drying oven.
[0065] In S2, the drying tunnel is a three-stage drying.
[0066] The first drying tunnel has a drying temperature of 80°C and a drying time of 1 minute; the second drying tunnel has a drying temperature of 120°C and a drying time of 2.5 minutes; the third drying tunnel has a drying temperature of 150°C and a drying time of 2.5 minutes.
[0067] Example 2
[0068] 1. A heat-activated protective adhesive for preventing collision and slipping, which is different from Example 1 in that:
[0069] The raw materials for preparing the product include, by mass percentage, 30% of ethyl acetate, 15% of xylene, 48% of polyurethane polymer, 6% of tackifying resin, 0.7% of filler and 0.3% of antioxidant.
[0070] 2. A method for preparing a collision-proof and anti-slip heat-activated protective adhesive, same as in Example 1.
[0071] Comparative Example 1
[0072] 1. A heat-activated protective adhesive for preventing collision and slipping, which is different from Example 1 in that:
[0073] The mass ratio of the polyoxypropylene ether polyol to the silane-modified polyether polyol is 1:2.5.
[0074] 2. A method for preparing a collision-proof and anti-slip heat-activated protective adhesive, same as in Example 1.
[0075] Comparative Example 2
[0076] 1. A heat-activated protective adhesive for preventing collision and slipping, which is different from Example 1 in that:
[0077] The weight ratio of the polyethylene adipate diol to the polyester polyol of 1,6-adipic acid / 1.6-hexanediol / neopentyl glycol is 0.5:1.
[0078] 2. A method for preparing a collision-proof and anti-slip heat-activated protective adhesive, same as in Example 1.
[0079] Comparative Example 3
[0080] 1. A heat-activated protective adhesive for preventing collision and slipping, which is different from Example 1 in that:
[0081] The terpene phenolic resin has an average molecular weight of 550, an acid value of less than 80 mgKOH / g, and a softening point of 120-135° C. (Shandong Guangshen Electronic Technology Co., Ltd., model 901).
[0082] 2. A method for preparing a collision-proof and anti-slip heat-activated protective adhesive, same as in Example 1.
[0083] Performance Testing
[0084] Sample processing: The thickness of the sample obtained in Example 1 was set to 0.24 mm (product 1) and 0.26 mm (product 2), and 6 pieces of 50 mm*200 mm were cut respectively. The protective film on the surface was removed and placed in an oven at 100°C for 1 hour. After that, the samples were taken out and left for a period of time to return to room temperature. The samples were placed on a roller at 180°C for thermal bonding. Figure 1 As shown, the bonding time is two time periods of 5s and 10s.
[0085] 1. 80℃ displacement test: Take two of them and do the displacement test with the platform temperature of 80℃. Specifically, heat the platform at 80℃, press the tape and the aluminum sheet for 5s and 10s respectively, then fix the tape, hold one end of the aluminum sheet with a screwdriver, push forward, and observe the displacement. The specific results are as follows: Figure 2 , 3 shown.
[0086] As can be seen from the figure, there is no relative displacement between Sample 1 and Sample 2 after being pressed for 5s and 10s, indicating that the protective adhesive can be activated at 80°C and has high bonding strength.
[0087] 2. Peeling force test: The other 4 pieces of sample 1 and sample 2 were tested for the peeling force performance of the tape using an electronic tensile testing machine according to the requirements of GB / T2792-2014. The specific results are shown in Table 1. Figure 4 and 5 shown.
[0088] In Example 1, the 5s pasted are numbered 1-4, and the 10s pasted are numbered 9-12; in Example 2, the 5s pasted are numbered 5-8, and the 10s pasted are numbered 13-16.
[0089] Width (outer width): It is the width of the aluminum sheet bonded with the tape during the test. The size of the aluminum sheet is 25mm*100mm.
[0090] Table 1 Peel force test results of Example 1 and Example 2
[0091]
[0092] The sample with test number 1 was significantly lower than other parallel samples due to an error in the sample bonding process, so it was discarded in the subsequent calculations.
[0093] It can be seen from the test data that both products have high strength, the 0.26mm thickness has higher peeling force and good heat resistance.
[0094] 3. The samples obtained from the embodiments and comparative examples were tested, the thickness of the test number was 0.26 mm, and the test results are shown in Table 2.
[0095] In the average value of the peeling interval load / N, Example 1 is the average value of serial numbers 2-4, and and are the average values of four groups of data.
[0096] Table 2 Test results of samples obtained from examples and comparative examples
[0097]
Claims
1. A heat-activated protective adhesive for anti-collision and anti-slip properties, characterized in that: The raw materials for its preparation, by mass percentage, include: Ethyl acetate 25-35%, xylene 15-25%, polyurethane polymer 40-50%, tackifying resin 5-15%, filler 0.5-2%, antioxidant 0.1-1%; The raw materials for preparing the polyurethane polymer include polyester polyol, polyether polyol, isocyanate, hydrophilic chain extender and catalyst; The polyester polyol is a polyester polyol of polyethylene adipate glycol and 1,6-adipic acid / 1,6-hexanediol / neopentyl glycol; The weight ratio of the polyethylene adipate diol to the polyester polyol of 1,6-adipic acid / 1,6-hexanediol / neopentyl glycol is 1.6:1; The polyether polyol is polypropylene oxide ether polyol and silane-modified polyether polyol; The mass ratio of the polyoxypropylene ether polyol to the silane-modified polyether polyol is 1:1.2; The isocyanate is diphenylmethane diisocyanate and hexamethylene diisocyanate; The mass ratio of diphenylmethane diisocyanate to hexamethylene diisocyanate is 1:1; The hydrophilic chain extender is N-butyl diethanolamine and dimethylol butyric acid; The mass ratio of the N-butyl diethanolamine to dimethylol butyric acid is 1:2.3; The tackifying resin is a terpene phenolic resin; The terpene phenolic resin has an average molecular weight of 690, an acid value of 45 to 60 mgKOH / g, and a softening point of 145 to 160°C; The filler is calcium carbonate; the calcium carbonate is heavy calcium carbonate; the average particle size of the heavy calcium carbonate is 800 meshes.
2. A method for preparing the anti-collision and anti-slip heat-activated protective adhesive according to claim 1, characterized in that: It includes the following steps: S1. After mixing the prepared raw materials, apply them once on the upper surface of the PET substrate; S2. The sample obtained in S1 is dried in a drying oven to obtain; In S2, the drying tunnel is a three-stage drying.