Preparation of needle-like core-shell nitride-oxide composites by urea method and their application in water electrolysis
The preparation of acupuncture core-shell structure nitride-oxide composites through the urea method solved the problems of slow OER kinetics and poor ammonia use, and achieved efficient electrocatalytic oxygen evolution performance and stability, with industrial application prospects.
Patent Information
- Application Number
- CN202310016518.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-06
AI Technical Summary
The oxidative electrolysis reaction (OER) of the four electron transfer steps has slow kinetics and low energy conversion efficiency in electrocatalytic water decomposition, resulting in bottlenecks in the entire water electrolysis process. The existing metal nitride synthesis methods are highly corrosive and environmentally friendly. Friendly ammonia as nitrogen source.
The urea method is used to prepare acupuncture core-shell structure nitride-oxide composites. By combining hydrothermal method and high-temperature thermal nitriding method, solid urea is used as nitrogen source to form a nanoneedle structure to enhance catalytic active site exposure and electrons Transport efficiency and exhibit high catalytic stability under alkaline conditions.
The high-efficiency electrocatalytic oxygen evolution performance under alkaline conditions was achieved. The overpotentials of the acupuncture core-shell structure nitride-oxide composite at 10mA/cm² and 100mA/cm² current density were 173mV and 282mV, respectively, and in large quantities It maintains stable operation for 20 hours at current density, and has industrial application prospects.
Smart Images

Figure CN115852431B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation and application of electrocatalysts, and more specifically, to the application of a needle-shaped core-shell structured nitride-oxide composite material in the field of electrocatalytic water splitting. Background Art
[0002] Electrocatalytic water splitting is the most promising technology for hydrogen production in the future. The electrocatalytic water splitting process involves two important half reactions, namely the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Both half reactions require catalysts to reduce the overpotential and improve the reaction efficiency. However, the four-electron transfer step of OER is the bottleneck of the entire water electrolysis due to its inherently slow kinetics and low energy conversion efficiency. Transition metal oxides have been developed as efficient OER catalysts in alkaline media due to their good conductivity and excellent catalytic performance. However, nanostructure control with specially designed surfaces, such as forming core-shell structures to facilitate active site exposure and charge transfer, is more desirable. Metal nitrides allow faster charge carrier transport and better conductivity than their oxides, which helps catalysis.
[0003] The current mainstream method for synthesizing metal nitrides is to use ammonia as a nitrogen source, but ammonia is highly corrosive, environmentally unfriendly, and has a strong irritating odor. Compared with the current mainstream sheet-like and block-like nitride catalysts, the needle-like structure has a larger specific surface area and can expose more active sites. The present invention uses the urea method to prepare a needle-like core-shell structure nitride-oxide composite material, using solid urea as a nitrogen source, the experimental conditions are relatively loose, and the degree of nitridation can be controlled by controlling the quality of urea to form a needle-like core-shell structure that is more conducive to catalysis, and the unique interfacial force of the needle-like core-shell structure can also promote the transmission of electrons. At the same time, the needle-like core-shell structure nitride-oxide composite material prepared by this method has a higher electrocatalytic water splitting performance, and shows high catalytic stability under alkaline conditions, and has a strong prospect for industrial application. Summary of the invention
[0004] The first object of the present invention is to provide a method for preparing a needle-shaped core-shell structured nitride-oxide composite material by a urea method.
[0005] The second purpose of the present invention is to provide an application of a urea method for preparing a needle-shaped core-shell structured nitride-oxide composite material.
[0006] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0007] The present invention discloses a method for preparing a core-shell structured nitride-oxide composite material by a urea method, comprising the following steps:
[0008] Step 1: Prepare metal oxide precursor materials by hydrothermal method.
[0009] Step 2: Place the precursor in a tube furnace and use a high-temperature thermal nitridation method to nitride the surface to obtain a core-shell structured nitride-oxide composite material.
[0010] A method for preparing a needle-shaped core-shell structure nitride-oxide composite material by a urea method, wherein the needle-shaped core-shell structure nitride-oxide composite material presents a nano needle structure with a diameter of 50nm-200nm and a surface nitride layer thickness of 10nm-30nm.
[0011] Furthermore, the specific operation of the hydrothermal method is: adding the metal source, urea and ammonium fluoride into deionized water and stirring evenly, reacting the mixed solution and the substrate under hydrothermal conditions, taking out the substrate after the reaction, repeatedly rinsing it with ethanol and deionized water, and drying it.
[0012] Furthermore, the nitrogen source of the high temperature thermal nitridation method is urea;
[0013] Furthermore, the specific operation of the high-temperature thermal nitridation method is: placing urea in a quartz boat, placing carbon felt on urea, placing a metal oxide precursor on the carbon felt, placing the quartz boat in a quartz tube, placing the quartz tube in a tubular furnace, introducing argon or nitrogen, raising the tubular furnace to the reaction temperature and keeping it warm, and then cooling it to room temperature.
[0014] Furthermore, the metal source is one of copper nitrate, cobalt nitrate and nickel nitrate, and the substrate is nickel foam.
[0015] Furthermore, the molar number of the metal source is 2 mmol-8 mmol.
[0016] Furthermore, the high temperature thermal nitriding method is carried out at 200°C-500°C for 1-4 hours.
[0017] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0018] The invention discloses application of a needle-shaped core-shell structure nitride-oxide composite material prepared by a urea method in electrocatalytic water decomposition.
[0019] Furthermore, the needle-shaped core-shell structured nitride-oxide composite material is used as an electrocatalyst for the electrolysis of water to produce oxygen under alkaline conditions. -2 and 100mA cm -2 When , the overpotential of the nitride-oxide composite electrocatalyst in alkaline electrolyte is 173 mV and 282 mV respectively.
[0020] Compared with the currently disclosed technology, the urea method of the present invention for preparing needle-shaped core-shell structure nitride-oxide composite materials has the following advantages:
[0021] (1) The unique needle-shaped core-shell structure has uniform morphology, large specific surface area, and good conductivity. It can increase the contact area with the electrolyte and expose more active sites. In addition, the unique interfacial force of the needle-shaped core-shell structure can also promote the transmission of electrons.
[0022] (2) The prepared electrocatalyst electrode has excellent electrocatalytic oxygen evolution performance under alkaline conditions. Comparing samples nitrided at different temperatures, taking cobalt as the metal source as an example, the performance is best at 300°C, with an overpotential of 173 mV at a current density of 10 mA and an overpotential of 282 mV at a high current density (100 mA).
[0023] (3) The prepared needle-shaped core-shell structured nitride-oxide composite electrode has good stability. When subjected to a chronoamperometric test at a current density of 100 mA, its constant voltage remained almost unchanged after 20 hours of stable operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Co prepared in Example 1 of the present invention 5.47 XRD pattern of N-CoO / NF electrode.
[0025] Figure 2 Co prepared in Example 1 of the present invention 5.47 SEM image of N-CoO / NF electrode.
[0026] Figure 3 Co prepared in Example 1 of the present invention 5.47 TEM image of N-CoO / NF electrode.
[0027] Figure 4 Co prepared in Example 1 of the present invention 5.47 OER performance diagram of N-CoO / NF electrode.
[0028] Figure 5 This is the OER performance diagram of the Cu3N-CuO / NF electrode prepared in Example 2 of the present invention.
[0029] Figure 6 This is the OER performance diagram of the Ni3N-NiO / NF electrode prepared in Example 3 of the present invention.
[0030] Figure 7 Co prepared in Example 4 of the present invention 5.47 OER performance diagram of N-CoO / NF electrode.
[0031] Figure 8This is the XRD diagram of the electrode prepared in Comparative Example 1 of the present invention.
[0032] Fig. 9 Co prepared in Example 1 of the present invention 5.47 Stability test diagram of N-CoO / NF electrode. DETAILED DESCRIPTION
[0033] In some typical embodiments, the hydrothermal method for synthesizing a metal precursor is as follows: adding a metal source, urea and ammonium fluoride into deionized water and stirring evenly, reacting the mixture with a substrate under hydrothermal conditions, taking out the substrate after the reaction, repeatedly rinsing it with ethanol and deionized water, and drying it.
[0034] In some typical embodiments, the method for preparing the needle-shaped core-shell structure nitride-oxide composite material by the urea method is as follows: urea is placed in a quartz boat, carbon felt is placed on the urea, a metal oxide precursor is placed on the carbon felt, the quartz boat is placed in a quartz tube, and the quartz tube is placed in a tube furnace. Argon or nitrogen is introduced, the tube furnace is raised to the reaction temperature and kept warm, and then cooled to room temperature.
[0035] In some typical embodiments, the substrate is nickel foam.
[0036] In some typical embodiments, the nickel foam cleaning step is: ultrasonically cleaning the nickel foam in dilute hydrochloric acid, acetone, and deionized water for 15 minutes, and then vacuum drying and preserving the cleaned nickel foam.
[0037] In some typical embodiments, the metal source is nickel nitrate, copper nitrate, cobalt nitrate, or the like.
[0038] In some typical embodiments, the thermal nitridation conditions are: heating at 200° C.-500° C. for 1-4 hours.
[0039] In some typical embodiments, the molar number of the metal source is 2 mmol-8 mmol.
[0040] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0041] Example 1
[0042] A urea method for preparing Co 5.47 The method of N-CoO / NF composite material comprises the following steps:
[0043] (1) Substrate cleaning: Take a 2 cm × 4 cm × 0.15 cm nickel foam and place it in 1 M dilute hydrochloric acid, acetone and ethanol in turn, and ultrasonically clean each for 15 minutes. Place the cleaned nickel foam in a vacuum oven and dry it for later use.
[0044] (2) Preparation of CoO / NF precursor by hydrothermal method:
[0045] Take 2 mmol of cobalt nitrate hexahydrate, 20 mmol of urea and 8 mmol of ammonium fluoride and dissolve them in 60 mL of water at room temperature to obtain a red solution. Transfer the solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, place the nickel foam in step (1) in the autoclave as a substrate, and place the autoclave in a 120°C oven for continuous heating for 6 h. After the reaction, cool naturally to room temperature, take out the nickel foam with the precursor, rinse it repeatedly with ethanol and deionized water, and then dry it in a vacuum drying oven to obtain the CoO / NF precursor.
[0046] (3) Preparation of Co by urea method 5.47 N-CoO / NF composites:
[0047] Take a quartz boat with a specification of 2.5cm×7.5cm, add 6g of urea, lay two layers of carbon felt on top of the urea, put the CoO / NF precursor obtained in step (2) on top of the carbon felt, put the quartz boat into a quartz tube, put the quartz tube into a tube furnace, pass argon as a protective gas, and then heat the tube furnace to 300℃ and keep it warm for 3 hours. After the temperature in the furnace cools naturally to room temperature, take out the sample, which is Co 5.47 N-CoO / NF composite material. The thickness of its nitride layer is about 20nm.
[0048] Example 2
[0049] A method for preparing a Cu3N-CuO / NF composite material by a urea process comprises the following steps:
[0050] (1) Substrate cleaning: same as in Example 1.
[0051] (2) Preparation of CuO / NF precursor by hydrothermal method:
[0052] Take 4 mmol of copper nitrate trihydrate, 20 mmol of urea and 8 mmol of ammonium fluoride and dissolve them in 60 mL of water at room temperature to obtain a blue solution. Transfer the solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, place the nickel foam in step (1) in the autoclave as a substrate, and place the autoclave in a 120°C oven and heat it continuously for 6 h. After the reaction, cool naturally to room temperature, take out the nickel foam with the precursor, rinse it repeatedly with ethanol and deionized water, and then dry it in a vacuum drying oven to obtain a CuO / NF precursor.
[0053] (3) Preparation of Cu3N-CuO / NF composite materials by urea method:
[0054] Take a quartz boat with a specification of 2.5 cm × 7.5 cm, add 6 g of urea to it, lay two layers of carbon felt on top of the urea, place the CuO / NF precursor obtained in step (2) on top of the carbon felt, put the quartz boat into a quartz tube, put the quartz tube into a tube furnace, pass argon as a protective gas, and then heat the tube furnace to 200°C and keep it warm for 4 hours. After the temperature in the furnace is naturally cooled to room temperature, take out the sample, which is the Cu3N-CuO / NF composite material. The thickness of its nitride layer is about 12 nm.
[0055] Example 3
[0056] A method for preparing a Ni3N-NiO / NF composite material by a urea process comprises the following steps:
[0057] (1) Substrate cleaning: same as in Example 1.
[0058] (4) Preparation of NiO / NF precursor by hydrothermal method:
[0059] Take 6 mmol nickel nitrate hexahydrate, 20 mmol urea and 8 mmol ammonium fluoride and dissolve them in 60 mL water at room temperature to obtain a turquoise solution. Transfer the solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, place the nickel foam in step (1) in the autoclave as a substrate, and place the autoclave in a 120°C oven and heat it continuously for 6 h. After the reaction, cool naturally to room temperature, take out the nickel foam with the precursor, rinse it repeatedly with ethanol and deionized water, and then dry it in a vacuum drying oven to obtain a NiO / NF precursor.
[0060] (1) Preparation of Ni3N-NiO / NF composite materials by urea method:
[0061] Take a quartz boat with a specification of 2.5 cm × 7.5 cm, add 6 g of urea, lay two layers of carbon felt on top of the urea, place the NiO / NF precursor obtained in step (2) on top of the carbon felt, put the quartz boat into a quartz tube, put the quartz tube into a tube furnace, pass argon as a protective gas, and then heat the tube furnace to 400°C and keep it warm for 2 hours. After the temperature in the furnace is naturally cooled to room temperature, take out the sample, which is the Ni3N-NiO / NF composite material. The thickness of its nitride layer is about 26 nm.
[0062] Example 4
[0063] A urea method for preparing Co 5.47 The method of N-CoO / NF composite material comprises the following steps:
[0064] (1) Substrate cleaning: same as in Example 1.
[0065] (2) Preparation of CoO / NF precursor:
[0066] Take 8 mmol of cobalt nitrate hexahydrate, 20 mmol of urea and 8 mmol of ammonium fluoride and dissolve them in 60 mL of water at room temperature to obtain a red solution. Transfer the solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, place the nickel foam in step (1) in the autoclave as a substrate, and place the autoclave in a 120°C oven for continuous heating for 6 h. After the reaction, cool naturally to room temperature, take out the nickel foam with the precursor, rinse it repeatedly with ethanol and deionized water, and then dry it in a vacuum drying oven to obtain the CoO / NF precursor.
[0067] (3) Preparation of Co by urea method 5.47 N-CoO / NF composites:
[0068] Take a quartz boat with a size of 2.5 cm × 7.5 cm, add 6 g of urea, lay two layers of carbon felt on top of the urea, place the CoO / NF precursor obtained in step (2) on top of the carbon felt, put the quartz boat into a quartz tube, put the quartz tube into a tube furnace, pass argon as a protective gas, and then heat the tube furnace to 500 ° C and keep it warm for 1 hour. After the temperature in the furnace cools naturally to room temperature, take out the sample, which is Co 5.47 N-CoO / NF composite material. The thickness of its nitride layer is about 22nm.
[0069] Comparative Example 1
[0070] The sample preparation method is the same as that of Example 1, except that the thermal nitridation temperature is 600° C. and maintained for 3 hours.
[0071] Performance Testing
[0072] Figure 1 Co prepared in Example 1 5.47 From the XRD diagram of N-CoO / NF composite material, we can see that the diffraction peak of nickel as the substrate is very strong. 5.47 The XRD patterns of N-CoO / NF composite materials correspond well to the standard card, which indicates that the synthesized material is Co 5.47 N structure, its three peaks correspond to the (1,1,1), (2,0,0), and (2,2,0) crystal planes respectively.
[0073] Figure 2 The Co prepared in Example 1 5.47 The SEM image of the N-CoO / NF composite electrode shows that the main body of the material is in the shape of nano needles. The morphology is uniform, which can expose more active sites and shorten the electron transmission distance.
[0074] Figure 3 Co prepared in Example 1 5.47TEM image of N-CoO / NF composite material shows that a single nanoneedle consists of an inner side (CoO) and an outer side (Co 5.47 The thickness of the nitride layer is about 20 nm, and the lattice spacing of (1,1,1) corresponding to the strongest peak is 0.206 nm, which is consistent with the XRD data.
[0075] Figure 4-7 The OER performance diagram of the needle-like core-shell structure nitride-oxide composite material prepared by the urea method is shown in Table 1. Since the needle-like core-shell structure can accelerate electron transfer, it can be seen that the core-shell structure nitride-oxide composite material synthesized by the urea thermal nitridation method has good OER performance. Among them, Co 5.47 N-CoO / NF electrode at 10 mA / cm 2 The overpotential under current density is 173mV. In addition, by comparison, it is not difficult to find that under the same current density, the overpotential of cobalt nitride is better than that of copper nitride and nickel nitride, indicating that cobalt ions have better OER performance than copper and nickel ions.
[0076] Table 1. Synthesis process and electrocatalytic data of Examples 1-4 and Comparative Example 1
[0077]
[0078] Figure 8 This is the XRD diagram of Comparative Example 1. It can be seen that the sample prepared by keeping warm at 600 degrees Celsius for 3 hours has only the peak of the base nickel foam, and no peak of cobalt nitride. It can be judged that the prepared sample is not a nitride. The reason is that urea will produce ammonia at 160 degrees Celsius, and ammonia will decompose into nitrogen and hydrogen when the temperature exceeds 500 degrees Celsius. After the ammonia decomposes, the precursor lacks a nitrogen source, so nitride will not be generated again when the temperature exceeds 500 degrees Celsius.
[0079] Fig. 9 The Co prepared in Example 1 was measured by chronoamperometry. 5.47 The stability of the N-CoO / NF electrode was tested. It can be seen that after working at a high current density (100 mA) for 20 hours, the current did not change much, which shows that the electrode can work stably at a high current density, proving that the catalyst has excellent stability.
[0080] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a needle-shaped core-shell structured nitride-oxide composite material by a urea method, characterized in that: The following steps are involved: Step 1: Take 2 mmol of cobalt nitrate hexahydrate, 20 mmol of urea and 8 mmol of ammonium fluoride and dissolve them in 60 mL of water at room temperature to obtain a red solution; transfer the solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, put nickel foam into the autoclave as a substrate, place the autoclave in a 120°C oven and heat it continuously for 6 h, cool it naturally to room temperature after the reaction, take out the nickel foam with the precursor, rinse it repeatedly with ethanol and deionized water, and then dry it in a vacuum drying oven to obtain CoO / NF precursor; Step 2: Take a quartz boat with a specification of 2.5 cm × 7.5 cm, add 6 g of urea to it, lay two layers of carbon felt on top of the urea, put the CoO / NF precursor obtained in step 1 on top of the carbon felt, put the quartz boat into a quartz tube, put the quartz tube into a tube furnace, pass argon as a protective gas, then heat the tube furnace to 300 ° C and keep it warm for 3 hours, wait for the temperature in the furnace to cool naturally to room temperature, and take out the sample, which is the needle-shaped core-shell structure nitride-oxide composite material Co 5.47 N-CoO / NF, the thickness of its surface nitride layer is 20nm.
2. The needle-shaped core-shell structured nitride-oxide composite material obtained by the preparation method according to claim 1, characterized in that: The needle-shaped core-shell structure nitride-oxide composite material presents a nano needle-shaped structure with a diameter of 50nm-200nm.
3. The use of the needle-shaped core-shell structure nitride-oxide composite material according to claim 2, characterized in that: The needle-shaped core-shell structure nitride-oxide composite material is used as an electrocatalyst for the electrolysis of water to produce oxygen under alkaline conditions.
4. The use according to claim 3, characterized in that: When the current density reaches 10 mA cm -2 and 100mA cm -2 When , the overpotential of the nitride-oxide composite electrocatalyst in alkaline electrolyte is 173 mV and 282 mV respectively.
Citation Information
Patent Citations
Multilevel structure transition metal nitride electrode material and preparation method thereof
CN109055976A
Controllable preparation of difunctional non-noble metal nitride catalyst and application in hydrogen production by high-current electrolysis of urea
CN113908870A
Non-Noble Metal-Nitride Based Electrocatalysts for High-Performance Seawater Splitting
US20220349066A1
Coral reef-like nickel phosphide-tungsten oxide nanocomposite, method for preparing the coral reef-like nickel phosphide-tungsten oxide nanocomposite and catalyst for electrochemical water splitting including the coral reef-like nickel phosphide-tungsten oxide nanocomposite
US20230002921A1
Metal oxide-carbon nitride composite material and preparation method and use thereof
WO2017012210A1