Preparation method of CoNiP-C / MXene composite negative electrode material

Through the preparation of CoNiP-C/MXene composite materials, the problems of low specific capacity and volume expansion of lithium-ion battery anode materials are solved, and high-performance lithium-ion battery anode materials are realized, extending battery life and improving material stability.

CN115863581BActive Publication Date: 2024-10-15YAOHE ERA (QINGDAO) ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211591336.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-15
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

The existing lithium-ion battery negative electrode material graphite has a low specific capacity, and metal phosphide has problems with volume expansion and low rate performance during the energy storage process, which limits its application.

Method used

Using the preparation method of CoNiP-C/MXene composite materials, ultra-fine metal organic framework Co/Ni-MOFs/MXene precursor is generated through ultrasonic microwave reaction, and hollow spherical CoNiP-C/MXene composite materials are obtained through phosphating heat treatment. The conductivity of MXene and the high capacity of metal phosphide are combined to form a high-performance lithium-ion battery anode material.

Benefits of technology

The hollow spherical structure alleviates the volume expansion during the lithium storage process, improves the lithium storage capacity and the cycle performance of the material, enhances the electron transmission speed, extends the battery life and improves the stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115863581B_ABST
    Figure CN115863581B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method of a CoNiP-C / MXene composite material, wherein an ultrafine metal organic framework Co / Ni-MOF is generated in situ between layers of multilayer MXene by means of a coordination regulator and ultrasonic microwave rapid nucleation, and a ligand is used to form a hydrogen bond with a MXene functional group to realize the self-assembly of a MOF template and MXene, and a spherical Co / Ni-MOFs / MXene precursor is obtained by atomization and liquid nitrogen freezing, and finally a CoNiP-C / MXene composite material is obtained by phosphating heat treatment. In the present invention, the embedding of ultrafine MOFs will expand the interlayer spacing of multilayer MXene, promote the embedding of more lithium ions, and the spherical hollow structure provides sufficient space for the volume change of the internal phosphide, thereby ensuring the stability of the composite material structure, and the outermost layer of MXene can cross-link the active substance to enhance the conductivity, improve the lithium ion diffusion rate, and extend the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material synthesis and energy technology, and specifically relates to a method for preparing a hollow heterostructure CoNiP-C / MXene composite negative electrode material. Background Art

[0002] Currently, most commercial lithium-ion batteries use graphite as negative electrode material, but graphite material has the disadvantage of low specific capacity, and its theoretical capacity is only 372mAh / g. Therefore, the development of new high-performance negative electrode materials is the key to the development of the next generation of high-energy density lithium-ion batteries. Metal phosphides have the advantages of ultra-high reversible capacity, good electron transfer rate and rate performance, and are new lithium-ion battery negative electrode materials worthy of in-depth study. However, this type of material will experience obvious volume expansion during the energy storage process, and the rate performance is low. The above problems limit the application of metal phosphides as negative electrode materials. Summary of the invention

[0003] The main purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a CoNiP-C / MXene composite material for a lithium ion battery.

[0004] To achieve the above object, the present invention provides a method for preparing a CoNiP-C / MXene composite negative electrode material for a lithium ion battery, comprising the following steps:

[0005] (1) dissolving nickel acetylacetonate and cobalt nitrate in a solvent, adding a multilayer MXene, and ultrasonicating for 0.5 to 5 hours, adding the above solution to a solvent containing a coordination modifier and an organic ligand, and vigorously magnetically stirring for 2 to 10 hours, placing the mixed solution in an ultrasonic microwave reactor, and ultrasonically reacting at 70 to 95° C. for 10 to 150 seconds to obtain a Co / Ni-MOFs / MXene precursor mixed solution with ultrafine hybrid MOFs embedded between layers;

[0006] (2) Wash the precursor mixture several times with N,N-dimethylformamide or methanol and deionized water to prepare a 0.5-10 mg / mL precursor mixture, subject it to strong ultrasound for 30-90 seconds and shear emulsification for 5-20 minutes, and then spray it into liquid nitrogen at -196°C in the form of droplets. After the liquid nitrogen evaporates and freeze-dries, a spherical Co / Ni-MOFs / MXene precursor can be obtained;

[0007] (3) In a nitrogen atmosphere, the spherical Co / Ni-MOFs / MXene precursor is mixed with sodium hypophosphite and calcined at a calcination temperature of 200 to 400 °C to obtain a hollow spherical CoNiP-C / MXene composite negative electrode material for lithium-ion batteries.

[0008] Preferably, the organic ligand in step (1) includes -OH and -O groups, which can form hydrogen bonds with the functional groups of MXene, which is beneficial to the anchoring of ultrafine MOFs on multilayer MXene.

[0009] Preferably, the organic ligand in step (1) comprises one or more of terephthalic acid, trimesic acid, cyclohexanedicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,6-pyridinedicarboxylic acid, and 2-pyridinecarboxylic acid.

[0010] Preferably, the solvent in step (1) comprises one or more of ethanol, methanol, deionized water, DMF, acetone, dimethyl sulfoxide, and cyclopentyl methyl ether.

[0011] Preferably, the coordination regulator in step (1) includes one or more of acetic acid, benzoic acid, lauric acid, and polyvinyl pyrrolidone.

[0012] Preferably, in step (1), the mass ratio of cobalt nitrate to nickel acetylacetonate is 1:(0.1-2), the mass ratio of cobalt nitrate to organic ligand is 1:(0.1-6), and the mass ratio of cobalt nitrate to coordination regulator is 1:(0.5-6).

[0013] Preferably, the MXene material used in step (1) comprises Ti 3 C 2 、Ti 2 C、Nb 2 C.V 2 C.Mo 2 One or more of C, the mass ratio of cobalt nitrate to MXene material is 1:(0.001~0.1).

[0014] Preferably, in step (2), the frequency of the strong ultrasound is 20 to 30 kHz, the power is 300 to 800 W, the rotation speed of the shear emulsification is 8000 to 12000 rpm, and the atomized droplet size is 100 to 1200 μm.

[0015] Preferably, in step (3), the mass ratio of the precursor to sodium hypophosphite is 1:(5-20), and the calcination conditions are: a heating rate of 1-10°C / min, and a calcination time of 1-5h.

[0016] Preferably, the ultrafine Co / Ni-MOF particles obtained in step (1) have a particle size of 10 to 50 nm.

[0017] Preferably, the spherical CoNiP-C / MXene composite negative electrode material has a particle size of 0.1 to 500 μm, a carbon content of 3 to 30 wt.%, a MXene interlayer spacing of 20 to 200 nm, a MXene layer thickness of 10 to 400 nm, and a specific surface area of ​​50 to 700 m 2 / g, and the pore diameter is 5 to 50 nm.

[0018] The inventive concept of the present invention is as follows:

[0019] MXene is a new type of two-dimensional material, which can generally be divided into multilayer MXene and few-layer MXene forms. When used as anode materials for lithium-ion batteries, it has the advantages of good conductivity and high lithium ion diffusion efficiency. However, the actual lithium storage capacity of multilayer MXene is lower than the theoretical capacity. The main reason is that multilayer MXene is stacked like pages of a book, and the gap between layers is too small to be fully utilized. Embedding a high-capacity second phase into the interlayer of multilayer MXene can effectively increase the lithium storage capacity of MXene. Therefore, through structural design and material composite modification, high-performance metal phosphide / MXene anode materials can be obtained.

[0020] In the present invention, a metal phosphide with high specific capacity is compounded with a highly conductive MXene material to obtain a high-performance negative electrode material for a lithium-ion battery. The MXene material is obtained by etching and stripping a MAX phase material with HF (or a mixed solution of LiF and concentrated HCl). The etched MXene material has surface functional groups such as -OH, -O, and -F, and typical ones are Ti 3 C 2 、Ti 2 C、Nb 2 C.V 2 C.Mo 2 C, etc., the upper layer of liquid after etching can harvest a few layers of MXene material, while the bottom layer is multi-layer MXene material.

[0021] In view of the shortcomings of metal phosphides and MXene in lithium storage, the present invention generates ultrafine metal organic framework Co / Ni-MOF in situ between the layers of multilayer MXene by means of coordination regulators and ultrasonic microwave rapid nucleation, and uses ligands to form hydrogen bonds with MXene functional groups to achieve self-assembly of MOF template and MXene, obtains spherical Co / Ni-MOFs / MXene precursors through atomization and liquid nitrogen freezing, and finally obtains spherical CoNiP-C / MXene composite materials through phosphating heat treatment. During the heat treatment process, metal phosphides crystallize and nucleate inside the hollow sphere, and the hollow structure provides sufficient space for the volume change of lithium storage, ensuring that the particle cycle process can maintain the integrity of the structure, and MXene provides particles with a certain toughness, which can play a protective and bridging role, thereby enhancing the electrochemical properties of metal phosphides.

[0022] The technical solution adopted by the present invention has the following advantages compared with the prior art:

[0023] 1. The present invention uses a hollow spherical structure to alleviate the volume expansion of the phosphide lithium storage process, thereby extending the battery life.

[0024] 2. Ultrafine CoNiP-C particles can expand the interlayer spacing of multilayer MXene, thereby improving the lithium storage capacity of the composite material.

[0025] 3. MXene materials can stabilize and bridge phosphide particles, reduce side reactions between phosphides and electrolytes, and enhance the transmission speed of electrons, thereby improving material rate performance and improving material lithium storage stability.

[0026] 3. The CoNiP-C / MXene composite negative electrode material prepared by the present invention has strong cycle performance, and the reversible capacity can reach more than 750 mAh / g after 300 cycles at a high current density of 200 mA / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the SEM image of the CoNiP-C / MXene composite negative electrode material in Example 1. DETAILED DESCRIPTION

[0028] In order to better understand the present invention, the present invention is further described below through specific implementation methods, but the enumerated embodiments do not limit the protection scope of the present invention.

[0029] Example 1

[0030] A method for preparing a CoNiP-C / MXene composite negative electrode material for a lithium-ion battery, the specific steps are as follows:

[0031] (1) Weigh 10 mg of cobalt nitrate and 1 mg of nickel acetylacetonate and dissolve them in 50 ml of methanol. Then add 0.05 mg of multilayered Ti 3 C 2 , ultrasonically treated for 1 hour, the above solution was added to a mixed solution of ethanol and DMF containing 20 mg of 1,4-naphthalene dicarboxylic acid and 30 mg of trimesic acid, and strongly magnetically stirred for 3 hours, the mixed solution was placed in an ultrasonic microwave reactor, and ultrasonic microwave reaction was performed at 90°C for 100 seconds to obtain a Co / Ni-MOFs / MXene precursor mixed solution with ultrafine MOFs embedded in the interlayer;

[0032] (2) The precursor mixture was washed with deionized water and DMF for 5 times to prepare a 0.7 mg / mL precursor mixture, and subjected to strong ultrasound (20 kHz, 300 W) for 80 seconds and shear emulsification treatment at 10000 rpm for 10 minutes. The mixture was then sprayed into liquid nitrogen (-196 ° C) in the form of 500 μm droplets. After the liquid nitrogen evaporated and freeze-dried, a spherical Co / Ni-MOFs / MXene precursor was obtained.

[0033] (3) 30 mg of the precursor was mixed with 160 mg of sodium hypophosphite and calcined at a heating rate of 5 °C / min, a calcination temperature of 300 °C, a calcination time of 3 h, and a calcination atmosphere of nitrogen. After the furnace was cooled to room temperature, a spherical CoNiP-C / MXene material was obtained with a particle size of 2 μm, a carbon content of 10%, a MXene layer thickness of 30 nm, and a BET test specific surface area of ​​221 m 2 / g, pore distribution is 5~20nm.

[0034] The SEM image of the CoNiP-C / MXene material prepared in this example is as follows: Figure 1 shown.

[0035] Electrochemical performance test: The prepared electrode material was mixed with acetylene black and PVDF in a mass ratio of 8:1:1, and an appropriate amount of N-methylpyrrolidone was added to dissolve it. The slurry was coated on copper foil to prepare an electrode. The test electrode was dried in a vacuum oven at 110°C for 24 hours, and LiPF was added in a high-purity argon atmosphere glove box with EC / DEC / DMC=1:1:1 (volume ratio). 6 As electrolyte, glass fiber filter paper as liquid absorption membrane, PP film as separator, and lithium metal as battery negative electrode, assembled into 2016 button cell. Discharge and charge conditions: discharge to 0.02V and then charge to 3V at the same current density, and the selected current density is 200mA / g. The above battery was tested, and the reversible capacity remained at 768mAh / g after 300 cycles, indicating that the CoNiP-C / MXene material has good capacity retention and cycle stability.

[0036] Example 2

[0037] A method for preparing a CoNiP-C / MXene composite negative electrode material for a lithium-ion battery, the specific steps are as follows:

[0038] (1) Weigh 10 mg of cobalt nitrate and 10 mg of nickel acetylacetonate and dissolve them in 50 ml of a mixture of methanol and water. Then add 0.1 mg of multilayered V 2 C, ultrasonically treat for 3 hours, add the above solution to a cyclopentyl methyl ether solution containing 60 mg of polyvinyl pyrrolidone and 50 mg of cyclohexanedicarboxylic acid, stir vigorously with magnetic force for 8 hours, place the mixed solution in an ultrasonic microwave reactor, and react with ultrasonic microwave at 80°C for 90 seconds to obtain a Co / Ni-MOFs / MXene precursor mixed solution with ultrafine MOFs embedded in the interlayer;

[0039] (2) The precursor was washed with deionized water and methanol for 5 times to prepare a 5 mg / mL precursor mixture, and subjected to strong ultrasound (30 kHz, 800 W) for 50 seconds and shear emulsification at 9500 rpm for 15 minutes. The mixture was then sprayed into liquid nitrogen (-196 °C) in the form of 300 μm droplets. After the liquid nitrogen evaporated and freeze-dried, a spherical Co / Ni-MOFs / MXene precursor was obtained.

[0040] (3) 30 mg of the precursor was mixed with 300 mg of sodium hypophosphite and calcined at a heating rate of 6 °C / min, a calcination temperature of 350 °C, a calcination time of 5 h, and a calcination atmosphere of nitrogen. After the furnace was cooled to room temperature, a spherical CoNiP-C / MXene material was obtained with a particle size of 10 μm, a carbon content of 18%, a MXene layer thickness of 100 nm, and a BET test specific surface area of ​​351 m 2 / g, pore distribution is 5~40nm.

[0041] Electrochemical performance test: The electrochemical test of this example is the same as that of Example 1, and the reversible capacity is maintained at 780.2 mAh / g, indicating that the CoNiP-C / MXene material has good capacity retention and cycle stability.

[0042] Comparative Example

[0043] The CoNiP material for lithium-ion batteries is prepared by smelting method. The specific steps are as follows:

[0044] (1) Weigh 3 g of cobalt powder, 2.5 g of nickel powder, and 8 g of red phosphorus, mix them, and pour them into a crucible.

[0045] (2) The crucible of step (1) was calcined in a nitrogen atmosphere at 700° C. for 8 h. The CoNiP material was obtained after the furnace was cooled and ground through a 400-mesh sieve.

[0046] Electrochemical performance test: The electrochemical performance test of this comparative example is the same as that of Example 1. The reversible capacity of the CoNiP material after 300 cycles at a current density of 200 mA / g is 50.2 mAh / g.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a CoNiP-C / MXene composite negative electrode material, characterized in that: The following steps are involved: (1) dissolving nickel acetylacetonate and cobalt nitrate in a solvent, adding a multilayer MXene, and ultrasonicating for 0.5 to 5 hours, adding the above solution to a solvent containing a coordination modifier and an organic ligand, and vigorously magnetically stirring for 2 to 10 hours, placing the mixed solution in an ultrasonic microwave reactor, and ultrasonically reacting at 70 to 95° C. for 10 to 150 seconds to obtain a Co / Ni-MOFs / MXene precursor mixed solution with ultrafine hybrid MOFs embedded between layers; (2) Wash the precursor mixture several times with N,N-dimethylformamide or methanol and deionized water to prepare a 0.5-10 mg / mL precursor mixture, subject it to strong ultrasound for 30-90 seconds and shear emulsification for 5-20 minutes, and then spray it into liquid nitrogen at -196°C in the form of droplets. After the liquid nitrogen evaporates and freeze-dries, a spherical Co / Ni-MOFs / MXene precursor can be obtained; (3) In a nitrogen atmosphere, the spherical Co / Ni-MOFs / MXene precursor is mixed with sodium hypophosphite and calcined at a calcination temperature of 200 to 400 °C to obtain a hollow spherical CoNiP-C / MXene composite negative electrode material for lithium-ion batteries.

2. The preparation method according to claim 1, characterized in that The organic ligands in step (1) include -OH and -O groups, which can form hydrogen bonds with the functional groups of MXene.

3. The preparation method according to claim 2, characterized in that: The organic ligand in step (1) includes one or more of terephthalic acid, trimesic acid, cyclohexanedicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,6-pyridinedicarboxylic acid, and 2-pyridinecarboxylic acid.

4. The preparation method according to claim 1, wherein the solvent in step (1) comprises one or more of ethanol, methanol, deionized water, DMF, acetone, dimethyl sulfoxide, and cyclopentyl methyl ether.

5. The preparation method according to claim 1, characterized in that: The coordination regulator in step (1) includes one or more of acetic acid, benzoic acid, lauric acid, and polyvinyl pyrrolidone.

6. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of cobalt nitrate to nickel acetylacetonate is 1:(0.1-2), the mass ratio of cobalt nitrate to organic ligand is 1:(0.1-6), and the mass ratio of cobalt nitrate to coordination regulator is 1:(0.5-6).

7. The preparation method according to claim 1, characterized in that: The MXene material used in step (1) includes one or more of Ti3C2, Ti2C, Nb2C, V2C, and Mo2C, and the mass ratio of cobalt nitrate to MXene material is 1:(0.001-0.1).

8. The preparation method according to claim 1, characterized in that: In step (2), the frequency of the strong ultrasound is 20-30 kHz, the power is 300-800 W, the rotation speed of the shear emulsification is 8000-12000 rpm, and the droplet size is 100-1200 μm.

9. The preparation method according to claim 1, characterized in that: In step (3), the mass ratio of the precursor to sodium hypophosphite is 1:(5-20), and the calcination conditions are: a heating rate of 1-10°C / min, and a calcination time of 1-5h.