A composite modifier for improving the barrier properties of biodegradable films and a preparation method thereof

By using fillers such as nanogas phase silica and nano calcium carbonate in biodegradable materials, combined with silane coupling agent and oxidized polyethylene wax, the microstructure of the material is improved, and the moisture permeability problem of the biodegradable material film to water molecules is solved. Improves barrier performance and is suitable for humidity-sensitive packaging fields.

CN115873383BActive Publication Date: 2024-11-22JIANGSU JITRI MOLECULAR ENG INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211241458.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-11
Publication Date
2024-11-22
Estimated Expiration
2042-10-11

AI Technical Summary

Technical Problem

The existing biodegradable films have poor barrier properties to water molecules, resulting in high moisture permeability and are difficult to apply in the field of humidity-sensitive packaging.

Method used

Nanovas-phase silica and nano-calcium carbonate as fillers, combined with silane coupling agent and oxidized polyethylene wax, and through high-speed stirring and twin-screw extruder granulation technology, composite modifiers are formed to improve the microstructure of the material and Sealing properties enhance the barrier properties of biodegradable membranes.

Benefits of technology

It significantly reduces the moisture permeability of biodegradable films, improves the anti-permeability and strength of the material, and is suitable for humidity-sensitive packaging fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003884937710000021
    Figure BDA0003884937710000021
  • Figure BDA0003884937710000061
    Figure BDA0003884937710000061
Patent Text Reader

Abstract

The present invention provides a composite modifier for improving the barrier property of a biodegradable film and a preparation method thereof, and belongs to the technical field of biodegradable films. The present invention adopts PBAT 20-46%, PLA 10-35%, nano-fumed silica 18-30%, nano-calcium carbonate 12-20%, silane coupling agent 2-5%, and oxidized polyethylene wax 3-8% as raw materials, and obtains a composite modifier for improving the barrier property of a biodegradable film by extrusion granulation through a twin-screw extruder. The composite modifier of the present invention can change the microstructure of the biodegradable film without changing the functional groups of the biodegradable film itself, thereby improving the barrier property of the biodegradable film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable films, and in particular to a composite modifier for improving the barrier properties of biodegradable films and a preparation method thereof. Background Art

[0002] Biodegradable materials are alternative products to olefin-based polymer films that the country has vigorously advocated in recent years. Their excellent degradation performance is of epoch-making significance for solving the white pollution caused by plastic bags. It is an important measure taken by the Chinese government to achieve carbon peak and carbon neutrality in the future. However, at present, whether it is PBAT material or other types of biodegradable materials used for packaging films, there is a common disadvantage: poor barrier properties, especially barrier properties to water molecules, that is, the moisture permeability is relatively large, which is not conducive to packaging fields that are sensitive to humidity. The reason for this shortcoming is that biodegradable materials have more polar groups and are very compatible with water molecules with strong polarity, so water molecules can easily pass through the film, resulting in a high moisture permeability of biodegradable materials.

[0003] Among the existing biodegradable materials, PBAT and PLA are the most widely used. Other biodegradable materials with great development potential in the future include PBS, PHA, etc. These materials contain highly polar functional groups such as -OH, -COOH, and -COO-. These functional groups have a good affinity for water molecules, so water molecules can easily pass through the film and enter the internal space of the package, thereby affecting the internal humidity.

[0004] The patent with application number CN202011248988.5 discloses a fully biodegradable high-barrier PLA / PBAT composite packaging film, which utilizes the characteristics of modified nano-silica that can polymerize with modified graphene during the extrusion granulation process to form a tightly interwoven network structure, thereby improving the performance of the PLA / PBAT composite material in blocking oxygen and water vapor. However, the working principles of the patent and the present invention are different. First, the formula of the patent is different from that of the present invention. The formula of the patent also contains modified graphene, and the modification process of the modified nano-silica used is too complicated, which is not conducive to large-scale production by users or the production process is complicated and the cost is too high. Secondly, the patent provides a production process for the composite packaging film, while the present invention provides a formula and process for the modifier, and there are substantial differences between the two. Thirdly, the modified nano-silica used in the patent is a compound formed by the reaction of silicon dioxide and vinyltrimethoxysilane. From a chemical point of view, it can no longer be called "nano-silica". Similar PBAT is formed by copolymerizing adipic acid in the PET molecular chain, but we cannot call PBAT "modified PET". Summary of the invention

[0005] In view of this, the present invention provides a composite modifier for improving the barrier properties of biodegradable films and a preparation method thereof. The present invention selects appropriate types of modifiers to change the microstructure of the material without changing the functional groups of the biodegradable material molecules themselves, thereby achieving the purpose of improving the barrier properties of biodegradable materials and reducing the moisture permeability of biodegradable films.

[0006] The first object of the present invention is to provide a composite modifier for improving the barrier properties of biodegradable films, which comprises the following components in mass percentage:

[0007]

[0008] Preferably, the number average molecular weight of the PBAT (Chinese name: polybutylene adipate / terephthalate) is 100,000-120,000, and the molecular weight distribution index is 2.8-3.4.

[0009] Preferably, the number average molecular weight of the PLA (polylactic acid) is 430,000-470,000, and the molecular weight distribution index is 3.3-3.7.

[0010] Preferably, the particle size of the nano-fumed silica is 20-60 nm.

[0011] Preferably, the particle size of the nano calcium carbonate is 10-100 nm.

[0012] Preferably, the silane coupling agent is selected from at least one of silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570 and silane coupling agent LM-N308.

[0013] Preferably, the oxidized polyethylene wax is selected from at least one of low-density oxidized polyethylene wax and high-density oxidized polyethylene wax.

[0014] The functions of each substance are as follows:

[0015] (1) Nano-fumed silica has two functions. First, the serious lack of coordination on the surface of nano-fumed silica, the huge specific surface area and the lack of surface oxygen determine that it has extremely strong activity and can easily form bonds with the polar groups in the molecules of biodegradable materials, thereby increasing the binding force between molecules and acting as a barrier when water molecules enter the structure of biodegradable materials. Second, the high fluidity and small size effect of nano-fumed silica fills the space between polymer molecular chains, making the material denser, thereby improving the sealing and anti-permeability of the material.

[0016] (2) Nano-calcium carbonate molecules also have a similar mechanism of action as nano-fumed silica. There are also a large number of polar structures on the surface of nano-calcium carbonate particles, which can also form many bonding structures with the substrate, which can fill the pores left by nano-fumed silica.

[0017] (3) Both nanofiller particles have the effect of improving the strength of biodegradable materials.

[0018] (4) The addition of two biodegradable components, PBAT and PLA, aims to enable the two nanoparticles to fully bond with the biodegradable components and reduce the difficulty of later processing. At the same time, the compatibility of the material with different carriers can be adjusted by adjusting the ratio of the two biodegradable components.

[0019] (5) The role of silane coupling agent is to improve the compatibility of nano-fumed silica and nano-calcium carbonate with the two polar substrates PBAT and PLA, and to prevent the agglomeration of nano-material particles.

[0020] (6) The molecular chain of oxidized polyethylene wax carries a certain amount of polar groups such as carbonyl and hydroxyl groups, and has good compatibility with nano-silicon dioxide, nano-calcium carbonate, and polar resins PBAT and PLA. It also has coupling properties, which significantly improves the dispersion performance of inorganic powders in the resin.

[0021] The second object of the present invention is to provide a method for preparing a composite modifier for improving the barrier properties of biodegradable films, comprising the following steps:

[0022] (1) placing nano fumed silica, nano calcium carbonate powder, silane coupling agent and oxidized polyethylene wax in a high-speed mixer for stirring and kneading;

[0023] (2) adding PBAT and PLA into the high-speed mixer in step (1) and continuing to stir and mix;

[0024] (3) Extrusion granulation is carried out by melt blending in a twin-screw extruder at a temperature of 155-170° C. For uniform mixing, granulation is repeated three times to obtain a composite modifier for improving the barrier properties of the biodegradable film.

[0025] Preferably, the operating parameters of the twin-screw extruder for extrusion granulation in step (3) are: the temperatures of barrel zones 1 to 11 are 155°C, 158°C, 160°C, 162°C, 165°C, 167°C, 169°C, 170°C, 170°C, 168°C, and 166°C, respectively; the head temperature is 160°C; and the screw speed is 45-50rpm.

[0026] The third object of the present invention is to provide a method for preparing a biodegradable film, comprising the following steps: mixing PBAT, PLA and a composite modifier evenly, placing the mixture in a film blowing device and blowing the mixture into a biodegradable film.

[0027] Preferably, the mass percentages of the PBAT, PLA and composite modifier are 60-66%, 30-33% and 1-10%, respectively.

[0028] Preferably, the processing temperature of the blowing process is 140-150° C., and the thickness of the film is 0.05 mm.

[0029] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a suitable composition system, which can, on the one hand, bond with the original polar group to form a larger group, thereby hindering the movement of water molecules inside; on the other hand, fill the original internal gaps of the polymer, increase the density of the polymer, and prevent water molecules from penetrating through. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0031] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the raw materials and auxiliary agents are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0032] The number average molecular weight of PBAT used in the specific implementation mode of the present invention is 100,000-120,000, and the molecular weight distribution index is 2.8-3.4. The number average molecular weight of PLA is 430,000-470,000, and the molecular weight distribution index is 3.3-3.7.

[0033] The nano-fumed silica used in the specific implementation of the present invention has a particle size of 20-60nm, purchased from Hubei Huifu Nanomaterial Co., Ltd. and produced as HL-200. The nano-calcium carbonate used has a particle size of 10-100nm, purchased from Shanxi Lanhua Huaming Nanomaterial Co., Ltd. and produced as SP200.

[0034] The film blowing equipment used in the specific implementation mode of the present invention is a 3GSJ20*30 / FM200 film blowing machine unit customized by Dalian Plastic Machinery Factory.

[0035] The working parameters of the film blowing equipment used in the specific implementation mode of the present invention are as follows: the temperatures of barrel zones 1 to 6 are 145°C, 147°C, 149°C, 146°C, 144°C, and 145°C, respectively; the die temperature is 145°C; and the screw speed is 38 rpm.

[0036] The composite modifier 1 used in the following Examples 1-3 of the present invention is prepared according to the following steps:

[0037] (1) placing 18 wt% of nano-fumed silica, 20 wt% of nano-calcium carbonate powder, 5 wt% of a silane coupling agent and 7 wt% of a high-density oxidized polyethylene wax in a high-speed mixer and stirring and kneading them;

[0038] (2) adding 38 wt% of PBAT and 12 wt% of PLA into the high-speed mixer in step (1), and continuing to stir and mix;

[0039] (3) Under the temperature condition of 155-170°C, granulation is carried out by melt blending through a twin-screw extruder. In order to mix evenly, granulation is repeated 3 times. The working parameters of the twin-screw extruder for extrusion granulation are as follows: the temperatures of barrel zones 1 to 11 are 155°C, 158°C, 160°C, 162°C, 165°C, 167°C, 169°C, 170°C, 170°C, 168°C, and 166°C, respectively; the head temperature is 160°C; and the screw speed is 45-50rpm. Thus, a composite modifier for improving the barrier property of biodegradable films can be obtained.

[0040] The composite modifier 2 used in the following Examples 4-6 of the present invention is prepared according to the following steps:

[0041] (1) placing 30 wt% of nano-fumed silica, 12 wt% of nano-calcium carbonate powder, 2 wt% of a silane coupling agent and 6 wt% of a high-density oxidized polyethylene wax in a high-speed mixer and stirring and kneading them;

[0042] (2) adding 20 wt% of PBAT and 30 wt% of PLA into the high-speed mixer in step (1), and continuing to stir and mix;

[0043] (3) Under the temperature condition of 155-170°C, granulation is carried out by extrusion through a twin-screw extruder, and the operating parameters of the twin-screw extruder for extrusion granulation are as follows: the temperatures of barrel zones 1 to 11 are 155°C, 158°C, 160°C, 162°C, 165°C, 167°C, 169°C, 170°C, 170°C, 168°C, and 166°C, respectively; the head temperature is 160°C; and the screw speed is 45-50rpm, thereby obtaining a composite modifier for improving the barrier properties of biodegradable films.

[0044] Example 1

[0045] A method for preparing a biodegradable film, the specific preparation steps are as follows: 60wt% of PBAT, 30wt% of PLA, and 10wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0046] Example 2

[0047] A method for preparing a biodegradable film, the specific preparation steps are as follows: 62wt% of PBAT, 31wt% of PLA, and 17wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0048] Example 3

[0049] A method for preparing a biodegradable film, the specific preparation steps are as follows: 66wt% of PBAT, 33wt% of PLA, and 11wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0050] Example 4

[0051] A method for preparing a biodegradable film, the specific preparation steps are as follows: 60wt% of PBAT, 30wt% of PLA, and 10wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0052] Example 5

[0053] A method for preparing a biodegradable film, the specific preparation steps are as follows: 62wt% of PBAT, 31wt% of PLA, and 27wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0054] Example 6

[0055] A method for preparing a biodegradable film, the specific preparation steps are as follows: 66wt% of PBAT, 33wt% of PLA, and 21wt% of a composite modifier are mixed evenly, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0056] Comparative Example 1

[0057] A method for preparing a biodegradable film, the specific preparation steps are as follows: 60wt% of PBAT, 30wt% of PLA, and 10wt% of starch are uniformly mixed, placed in a film blowing device, and blown into a film with a thickness of 0.05mm at a temperature of 140°C.

[0058] Water vapor transmission rate test method:

[0059] Take a 100mL beaker, put 1g of anhydrous calcium chloride in it, cover the film sample on the mouth of the beaker, tie it with a rubber band, place the whole device in a constant temperature and humidity chamber at 35℃ and 100%RH. After natural moisture absorption for 48h, weigh it, obtain the amount of water absorbed by the inorganic salt, and calculate the water vapor permeability.

[0060] The biodegradable films prepared in Examples 1-6 and Comparative Example 1 were tested for water vapor transmission rate according to the above method. The test results are shown in Table 1:

[0061] Table 1

[0062]

[0063] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a composite modifier for improving the barrier properties of biodegradable films, It is characterized in that The following steps are involved: (1) placing nano-fumed silica, nano-calcium carbonate powder, silane coupling agent and oxidized polyethylene wax in a high-speed mixer and stirring and kneading them; (2) Add PBAT and PLA into the high-speed mixer in step (1) and continue stirring and mixing; (3) Extruding and granulating the mixture by melt blending in a twin-screw extruder at a temperature of 155-170°C. Repeating the granulation process three times to obtain a composite modifier for improving the barrier properties of the biodegradable film. The composite modifier comprises the following components in percentage by mass: PBAT 20-46% PLA 10-35% Nano fumed silica 18-30% Nano calcium carbonate 12-20% Silane coupling agent 2-5% Oxidized polyethylene wax 3-8%; The particle size of the nano calcium carbonate is 10-100 nm.

2. The method for preparing the composite modifier for improving the barrier properties of biodegradable films according to claim 1, It is characterized in that The number average molecular weight of the PBAT is 100,000-120,000, and the molecular weight distribution index is 2.8-3.

4.

3. The method for preparing the composite modifier for improving the barrier properties of biodegradable films according to claim 1, It is characterized in that The number average molecular weight of the PLA is 430,000-470,000, and the molecular weight distribution index is 3.3-3.

7.

4. The method for preparing the composite modifier for improving the barrier properties of biodegradable films according to claim 1, It is characterized in that The particle size of the nano-gas phase silica is 20-60nm.

5. The method for preparing the composite modifier for improving the barrier properties of biodegradable films according to claim 1, It is characterized in that The operating parameters of the twin-screw extruder for extrusion granulation in step (3) are as follows: the temperatures of barrel zones 1 to 11 are 155°C, 158°C, 160°C, 162°C, 165°C, 167°C, 169°C, 170°C, 170°C, 168°C, and 166°C, respectively; the die temperature is 160°C; and the screw speed is 45-50rpm.

6. A method for preparing a biodegradable film, It is characterized in that The following steps are involved: After PBAT, PLA and the composite modifier described in any one of claims 1 to 4 are uniformly mixed, the mixture is placed in a film blowing device and blown into a biodegradable film.

7. The method for preparing the biodegradable film according to claim 6, It is characterized in that The mass percentages of the PBAT, PLA and composite modifier are 60-66%, 30-33% and 1-10% respectively.

8. The method for preparing the biodegradable film according to claim 6, It is characterized in that The processing temperature of the blowing process is 140-150° C., and the thickness of the film is 0.05 mm.