A reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric and its preparation method and application

Through wet spinning technology, graphene oxide is compounded with dicyandiamide to form reduced graphene oxide/graphite-like phase carbon nitride composite nonwoven fabric, which solves the inadequate research on graphene one-dimensional assembly and the structural defects of graphene oxide fibers The problem of this paper has achieved improved conductivity and catalyticity, and improved the efficiency and stability of the electrode in lithium metal batteries.

CN115874357BActive Publication Date: 2024-12-06BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211640413.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-12-06
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

In the prior art, graphene one-dimensional macroscopic assembly has few researches, graphene oxide fiber structural defects, surface oxygen-containing functional groups hinder physical properties, graphite-like phase carbon nitride performance in the catalytic field is excellent, but the specific surface area is small, and the conductivity is Difference.

Method used

Wet spinning method is used to compound dicyandiamide and graphene oxide to form a reduced graphene oxide/graphite-like phase carbon nitride composite non-woven fabric, and graphene oxide/graphite-like phase carbon nitride is used to combine graphene oxide fibers and reduced graphene oxide/graphite-like phase carbon nitride Composite fibers overlap to form a multi-layer structure to enhance conductivity and catalyticity.

Benefits of technology

A material with good conductivity, catalyticity and processability is obtained, which is used for the negative electrode of lithium metal battery, induce uniform deposition of lithium ions, inhibit the growth of lithium dendrites, and improve the efficiency and circulation stability of Coulomb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115874357B_ABST
    Figure CN115874357B_ABST
Patent Text Reader

Abstract

Provided is a reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric and its preparation method and application. The nonwoven fabric is formed by overlapping reduced graphene oxide fibers and reduced graphene oxide / graphite-like carbon nitride composite fibers in a volume ratio of (2:1) to (1:1); the diameter range of the fiber is 30-70 μm. The preparation method comprises the following steps: S1, dispersing a monolayer of graphene oxide powder with N,N-dimethylformamide as a solvent to obtain a first dispersion; S2, preparing another dispersion in the same way, adding dicyandiamide powder, and stirring thoroughly to obtain a second dispersion; S3, spinning separately; then standing in a coagulation bath, filtering, soaking the mixed fiber in a saturated dicyandiamide acetone solution, sintering, and the like to obtain the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to the technical field of composite fiber materials, and specifically relates to a reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric and a preparation method and application thereof. Background Art

[0002] As a single-layer carbon allotrope, graphene has attracted much attention due to its unique physical and chemical properties, such as high electrical and thermal conductivity, large specific surface area and chemical stability. Some major progress has been made in its application in the fields of new energy, electronics, hydrogen storage, etc. These applications generally start with macroscopic assemblies of graphene. Generally, these composites have a large specific surface area, can serve as channels for fast electron transmission, increase carrier mobility, improve electrical conductivity, and are no less than other inorganic composites in terms of mechanical properties and thermal conductivity. In addition, this type of macroscopic assembly of graphene has other performance potentials to be explored and can be used in different application fields.

[0003] Among the numerous studies on graphene macroscopic assemblies, most of the research focuses on how to construct graphene films (2D) and graphene blocks (3D), which are limited by the irregular size and low monolayer rate of graphene itself, while there are fewer reports on one-dimensional graphene macroscopic assemblies.

[0004] The starting point of graphene macroscopic assemblies is generally graphene oxide. Since the liquid crystal arrangement behavior of graphene oxide in aqueous dispersions was discovered by domestic and foreign scholars, it has been shown that graphene oxide dispersions are spinnable and can be used to synthesize one-dimensional graphene oxide fibers through wet spinning. As an important method in the textile field, wet spinning has the advantages of simple operation, low requirements for the production environment, high degree of automation and large-scale preparation. The fabrics constructed by fibers have both structure and performance and can be used in multiple fields, such as catalysis and biosensing.

[0005] Single graphene oxide fiber has many structural defects, and the oxygen-containing functional groups on the surface will also hinder its physical properties. Generally, graphene oxide is converted into graphene or reduced graphene oxide by heat treatment, chemical reduction and other means. At this time, the defects of graphene oxide are removed, the functional groups are released, the structure is restored to a certain extent, and the physical properties are improved. At this time, it can be combined with some compounds to form composite graphene. Different from the doping of a single element, the composite product means the generation of a new phase, and the physical and chemical properties of the product can be a collection of multiple substances. Summary of the invention

[0006] The purpose of the present invention is to provide a reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric and its preparation method and application, dicyandiamide and graphene oxide are composited into composite fibers, and then graphene oxide fibers are used for lap joint, and finally carbonized to obtain a nonwoven fabric. Graphite-like carbon nitride (g-C3N4) has excellent performance in the field of catalysis, rich reaction sites, and some other excellent properties, but the specific surface area is very small, the conductivity is poor, and the processing performance is poor. Combining it with graphene or reduced graphene oxide, the two can complement each other to obtain a material with good conductivity, catalysis and processing properties.

[0007] The technical solution of the present invention is a reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric, characterized in that the non-woven fabric is formed by overlapping reduced graphene oxide / graphite-like carbon nitride composite fibers and reduced graphene oxide fibers to form a multilayer structure; the volume ratio of the reduced graphene oxide fibers to the reduced graphene oxide / graphite-like carbon nitride composite fibers is (2:1) to (1:1); the diameter range of the fibers is 30-70 μm.

[0008] The present invention also provides a method for preparing the above-mentioned reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric, comprising the following steps:

[0009] S1. Dispersing the monolayer graphene oxide powder uniformly with N,N-dimethylformamide as solvent, with the concentration of the dispersion being 10 to 20 mg / mL, to obtain a first dispersion;

[0010] S2, preparing a monolayer graphene oxide dispersion with the same concentration using the same method as step S1, adding dicyandiamide powder to the dispersed dispersion, and stirring thoroughly to obtain a second dispersion;

[0011] S3, performing wet spinning using the first dispersion and the second dispersion, wherein ethyl acetate is used as a coagulation bath for spinning; wherein the inner diameter of the needle for injecting the second dispersion is smaller than the inner diameter of the needle for injecting the first dispersion;

[0012] S4, placing the spun fiber obtained in step S3 in a coagulation bath to perform solvent exchange;

[0013] S5, filtering the mixture of step S4 on a Buchner funnel;

[0014] S6, soaking the two types of fibers after filtration in an acetone solution added with saturated dicyandiamide, and performing solvent exchange again;

[0015] S7, lightly stirring the mixture solution of step S6, and then filtering and collecting it with a filter screen, and the collected fibers are accumulated into a cake-like substance of a certain thickness;

[0016] S8, putting the collected cakes into an oven for drying;

[0017] S9, carbonizing the sample cut pieces dried in step S8 in a tube furnace, and naturally cooling to room temperature after carbonization to obtain the reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric.

[0018] Furthermore, the above step S1 includes a centrifugal separation step: the dispersion is subjected to one to three times of differential centrifugation, the centrifugal speed is controlled at 6000-12000 rpm, and the precipitate is taken and then dispersed with N,N-dimethylformamide.

[0019] Furthermore, in the above step S2, the mass ratio of dicyandiamide to the monolayer graphene oxide is (10:1) to (20:1).

[0020] Furthermore, the specific operation of the above step S3 is as follows: the first dispersion liquid is injected into the ethyl acetate coagulation bath with a rotation speed of 20 to 40 rpm at an injection speed of 80 to 500 μL / min; the second dispersion liquid is injected into the ethyl acetate coagulation bath at an injection speed of 50 to 300 μL / min.

[0021] Furthermore, in the above step S3, the inner diameter of the needle for injecting the first dispersion is 160 μm to 260 μm; the inner diameter of the needle for injecting the second dispersion is 60 μm to 160 μm; the ethyl acetate coagulation bath into which the second dispersion is injected is the same coagulation bath into which the first dispersion is injected or a separate coagulation bath with the same rotation speed as the ethyl acetate coagulation bath into which the first dispersion is injected.

[0022] Furthermore, in the above step S4, the spun fiber is placed in the coagulation bath for 10 to 180 minutes; in the step S6, the fiber is immersed in the acetone solution with saturated dicyandiamide for 10 to 180 minutes; in the above step S7, the filter is a metal filter or a plastic mesh.

[0023] Furthermore, in the above step S8, the drying temperature is 60-90°C; in the step S9, the temperature mechanism of carbonization is: the heating rate is 2-3°C / min, the carbonization temperature is 520-600°C, and the insulation time is 2-4h.

[0024] The present invention also provides an application of the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric, which can be used as a three-dimensional skeleton for the negative electrode in a lithium metal battery, and the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric serves as a substrate for lithium metal deposition. The results show that the skeleton can induce uniform deposition of lithium ions, inhibit the growth of lithium dendrites, and improve the coulombic efficiency and cycle stability of the metal electrode.

[0025] The advantages of the present invention compared to the prior art are:

[0026] 1) The non-woven fabric of the present invention includes two different fibers: Since graphene oxide has more oxygen-containing functional groups on its surface, the fibers can overlap and fuse with each other through similar dissolution, intermolecular forces, etc., and can form a non-woven fabric after spinning. However, if the inside or surface of the fiber is covered with salts such as dicyandiamide, it will be difficult to fuse the fibers. Therefore, after spinning the second dispersion formed by mixing the graphene oxide dispersion with dicyandiamide, the fibers are loose and cannot form a non-woven fabric. However, if the two types of fibers obtained by spinning are mixed, the graphene oxide fiber can enhance the fusion ability between the composite fibers, thereby promoting the formation of a non-woven fabric, and a non-woven fabric with certain flexibility and strength can be obtained.

[0027] 2) In the preparation method of the present invention, the inner diameters of the needles used for spinning the two types of fibers in the non-woven fabric are different: the spinning diameter of the reduced graphene oxide / graphite-like carbon nitride composite fiber is smaller than the spinning diameter of the reduced graphene oxide fiber. This is because the composite fiber generates g-C3N4 during the carbonization process and produces a large volume expansion, which will cause uneven stress distribution inside the non-woven fabric and structural damage. Therefore, a smaller composite fiber diameter is beneficial to maintaining the flexibility and strength of the non-woven fabric.

[0028] 3) In the preparation method of the present invention, a pretreatment process for improving the performance of the monolayer graphene oxide powder is designed: since the monolayer rate, oxidation degree and sheet size of graphene oxide have a great influence on the mechanical properties of the graphene oxide fiber, generally speaking, the fiber strength formed by a higher monolayer rate, a smaller oxidation degree and a larger sheet size is higher, and the graphene oxide fiber with better mechanical properties is crucial for the formation of non-woven fabrics, otherwise it is difficult to form non-woven fabrics or the formed non-woven fabrics shrink severely. Self-synthesized graphene oxide and commercially available graphene oxide are generally difficult to meet these parameter requirements. At this time, some pretreatments can be performed, such as chemical reduction or hydrothermal reduction, differential centrifugation, etc., which can improve the mechanical properties of graphene oxide fibers in the subsequent spinning process. The present invention uses differential centrifugation to screen the large flakes in the graphene oxide dispersion, because the ability of small flakes of graphene oxide to curl and form fibers is weak, resulting in poor fiber mechanical properties. The present invention uses a cell crusher and ultrasound to better disperse graphene oxide in the dispersion, and the subsequent spinning process will be smoother (so that the spinning needle is not blocked and the fiber mechanical properties are better). If the ultrasound power or ultrasound time is too large, large sheets of graphene oxide are easily destroyed by ultrasound and become smaller.

[0029] 4) In the application of the present invention, the reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric is applied as a lithium metal three-dimensional skeleton to the negative electrode in a lithium metal battery, which can induce uniform deposition of lithium and inhibit the growth of lithium dendrites, thereby improving the coulombic efficiency and cycle stability of the lithium metal electrode.

[0030] The present invention spins graphene oxide dispersion and mixed dispersion of graphene oxide and dicyandiamide respectively, and finally obtains reduced graphene oxide fiber and reduced graphene oxide / graphite-like phase nitrided carbon fiber composited in a certain proportion and in a certain form, thereby solving the problem that although g-C3N4 fiber has extremely excellent performance in the field of catalysis, it has very small specific surface area and poor electrical conductivity, and simultaneously solves the problem that single graphene oxide fiber itself has many structural defects and oxygen-containing functional groups on the surface will also hinder its physical properties. The combination of the two can complement each other and can significantly increase the application space in batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:

[0032] Figure 1 XRD curves of several samples related to Example 1 of the present invention;

[0033] Figure 2 This is the XPS curve of the nonwoven fabric obtained in Example 1 of the present invention;

[0034] Figure 3 The SEM images of the nonwoven fabric obtained in Example 1 of the present invention, wherein (a) and (b) are SEM images of the front side of the nonwoven fabric; (c) and (d) are SEM images of the cross section of the nonwoven fabric;

[0035] Figure 4 This is a surface SEM image of the non-woven fabric assembled half-cell of Example 1 after lithium deposition or cycling;

[0036] Figure 5 The test curve of the half-battery obtained from the nonwoven fabric of Example 1: at 1 mA / cm 2 The current density is 1 mAh / cm 2 Coulombic efficiency at capacity;

[0037] Figure 6 The test curve of the symmetrical battery based on the nonwoven fabric of Example 1: at 1 mA / cm 2 The current density is 1 mAh / cm 2 Stable cycle performance under the conditions of

[0038] Figure 7 The test curves of the full battery based on the non-woven fabric of Example 1 are as follows: (a) is the long cycle curve of the full battery assembled with the non-woven fabric prepared by wet spinning at 2C, with an initial lithium deposition amount of 3.5 mAh / cm 2, the positive electrode is lithium iron phosphate (LFP); (b) is the cycle curve of the full battery assembled by wet spinning non-woven fabric at different rates, with an initial lithium deposition amount of 3.5 mAh / cm 2 , the positive electrode is LFP;

[0039] Figure 8 The SEM images of the nonwoven fabrics obtained in Examples 2 and 3, wherein (a) is the nonwoven fabric obtained in Example 2; (b) is the nonwoven fabric obtained in Example 3;

[0040] Fig. 9 The BET test curve of the nonwoven fabric obtained in Example 1, wherein (a) the adsorption-desorption curve of the nonwoven fabric sample; (b) the pore size distribution curve of the nonwoven fabric sample;

[0041] Fig.10 These are morphological pictures of the nonwoven fabric obtained in Example 1 after being soaked for one week and then dried, wherein (a) is soaked in water; (b) is soaked in ethanol; (c) is soaked in DMF; (d) is soaked in acetic acid; and (e) is soaked in NMP. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0043] Example 1

[0044] A method for preparing a reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric comprises the following steps:

[0045] (1) A graphene oxide dispersion with a concentration of 12 mg / mL was prepared, and the solvent was N,N-dimethylformamide (DMF), which was dispersion 1. The same dispersion with a concentration of 12 mg / mL was prepared, and dicyandiamide powder was added thereto and stirred thoroughly. The mass ratio of dicyandiamide to graphene oxide powder was 15:1, which was dispersion 2.

[0046] (2) 2 mL of dispersion 1 was injected into a rotating ethyl acetate coagulation bath using a needle with an inner diameter of 160 μm at an injection speed of 150 μL / min, the coagulation bath rotation speed was 30 rpm, and the solution was allowed to stand for 1 h. 1.5 mL of dispersion 2 was injected into another rotating ethyl acetate coagulation bath using a needle with an inner diameter of 110 μm at an injection speed of 120 μL / min, the coagulation bath rotation speed was 30 rpm, and the solution was allowed to stand for 1 h.

[0047] (3) The two coagulation baths were then filtered through a Buchner funnel, and the fiber cake was placed in an acetone solution containing saturated dicyandiamide and soaked for 1 hour.

[0048] (4) Stir the solution slightly, collect the fiber cake through a copper mesh filter, and dry it in an oven at 80 degrees for 30 minutes.

[0049] (5) Finally, the non-woven fabric pieces were carbonized at a temperature of 550°C, a heating rate of 2°C / min, and a holding time of 3 h to obtain battery electrodes.

[0050] Among them, the XRD patterns of graphene oxide fiber (GO), reduced graphene oxide fiber (rGO), graphite-like carbon nitride fiber (g-C3N4), and reduced graphene oxide / graphite-like carbon nitride fiber (rGO / g-C3N4) are as follows: Figure 1 As shown: the (001) crystal plane of GO appears near 11.3°, and the corresponding crystal plane spacing is 0.782nm. At the same time, the plane spacing of the (002) crystal plane at 25.9° in rGO is 0.176nm. After the surface is heat treated, the functional groups in GO decompose and release small molecules. The repulsion between the sheets becomes smaller, and the spacing between the sheets is shortened. For g-C3N4, two characteristic peaks appear, which are the (100) crystal plane at 13.1° and the (002) crystal plane at 27.4°. The rGO / g-C3N4 sample also has two characteristic peaks, which can be regarded as the superposition result of the rGO curve and the g-C3N4 curve. They are located at 13° and 26.6°. The shift of the peak position indicates the formation of rGO / g-C3N4.

[0051] XPS of rGO / g-C3N4 Figure 2 As shown: The spectrum shows that the product contains three elements: C, N and O, among which the N content is about 16.35%, and the N element comes from g-C3N4.

[0052] The SEM scanning images of the obtained rGO / g-C3N4 fibers are shown in Figure 3 As shown: It can be seen that it is composed of single fibers, the diameter of a single fiber is about 50μm, and the fibers are cross-linked to form a rich three-dimensional network structure. Figure 3 (c) and (d) show the SEM images of the cross section of the nonwoven fabric. It can be seen that the nonwoven fabric has a layered structure and has a large number of wrinkles inside the fibers.

[0053] Fig. 9 is the BET test curve of the obtained nonwoven fabric, (a) is the adsorption-desorption curve of the sample with a hysteresis loop, which belongs to the IV type isotherm, which often appears in mesoporous multilayer materials and also corresponds to Figure 3 (c), subdivided into H3 type in type IV isotherm, H3 type curve is found in aggregates of layered structures, producing mesoporous or macroporous materials with narrow slits; Fig. 9 (b) The pore size distribution is concentrated in the range of 5-50 nm. The average pore size calculated by BJH is 26.2834 nm. The BET calculation results show that the surface area of ​​the sample is about 9.1569 m 2 / g, which is smaller than the specific surface area of ​​flaky graphene, indicating that the specific surface area decreases after graphene curls into fibers.

[0054] Fig.10 (a) to (e) are the morphology of the non-woven fabric after being immersed in water, ethanol, DMF, acetic acid and NMP for one week and then dried. It can be seen that the morphology is best maintained after being immersed in water and ethanol, and is slightly damaged in the other solutions. This indicates that the material is expected to be used in applications involving water, such as aqueous batteries, water purification, etc.

[0055] application:

[0056] The obtained non-woven fabric was cut into discs and used as the three-dimensional skeleton of the lithium metal electrode. They were assembled into half-cells, symmetrical cells and full cells (with lithium iron phosphate as the positive electrode) for battery cycle testing. The test principle is as follows:

[0057] For the assembled (asymmetric) half-cell, with a pure lithium sheet as the negative electrode and a sample electrode as the positive electrode, the reversibility of the deposition / stripping process of metallic lithium on the sample electrode can be characterized by the constant current charge and discharge method. The specific test method is to activate the battery first, first use a small current to cycle 5 times, and then conduct a formal test. During the formal test, first discharge with a certain constant current (lithium deposition), and then charge with the same current to the cut-off voltage (lithium stripping), and continue to cycle until the battery is damaged. The coulomb efficiency (CE) of the charge and discharge cycle is the ratio of the charging capacity to the discharge capacity.

[0058] For symmetrical cells, the symmetrical cell has the same structure as the half-cell, but a portion of metallic lithium is deposited on the sample electrode before the charge and discharge cycle is performed. After deposition, due to the presence of lithium metal at both the positive and negative electrodes of the battery, the voltage of the battery is close to 0V. As the number of charge and discharge cycles increases, the change in voltage can be clearly observed. The cycle stability of the metallic lithium negative electrode can be characterized by whether the voltage curve is stable. The entire test process is to first use a small current to cycle 5 times to activate the battery, and then deposit lithium on the positive electrode sample electrode. The subsequent tests are the same as the half-cell.

[0059] For the full battery, that is, the negative electrode is a sample electrode with lithium (obtained by pre-depositing lithium) and the positive electrode is lithium iron phosphate. First, it is activated for 3 cycles at a rate of 0.2C (Crate, the reaction charge and discharge speed), and then its cycle performance and rate performance are tested at different rates (0.2-10C). Among them, the constant current charge and discharge voltage range is 2.2~4.0V, that is, the discharge cut-off voltage is 2.2V, and the charge cut-off voltage is 4.0V.

[0060] The test results obtained can be found in Figure 4 , 5 , 6 and 7.

[0061] Figure 4 Surface SEM images of the nonwoven fabric assembled half-cell of Example 1 after lithium deposition or cycling: (a) shows a surface charge at 0.5 mA / cm 2 The morphology after lithium deposition for 1 h at a current density of 1 mA / cm2 shows that no obvious dendrites appear and the fiber diameter becomes significantly thicker; (b) shows that the fiber diameter becomes thicker at a current density of 1 mA / cm2. 2 The current density is 1 mAh / cm 2 After 100 cycles at a capacity of , the lithium deposition on the surface of the sample electrode is very uniform and smooth, and no lithium dendrites appear.

[0062] Figure 5 The test curve for half-cell: displayed at 1mA / cm 2 The current density is 1 mAh / cm 2 The experimental group can cycle more than 450 times with stable cycle performance at a capacity of , and the coulombic efficiency remains above 98.8%.

[0063] Figure 6 The test curve of the symmetrical battery shows that it can be operated at 1 mA / cm 2 、1mAh / cm 2 The battery can be cycled for more than 560 hours under the test conditions, and the overpotential is only about 21mv.

[0064] Figure 7 The test curve of the whole battery: (a) shows the long cycle 2C rate test of the whole battery. At the beginning of the cycle, the capacity can reach 126.2mAh / g, the coulomb efficiency of each cycle is above 99.5%, and the capacity retention rate after 1000 cycles is 78.6%; (b) shows its rate performance, testing the cycle performance of the whole battery at 0.2C to 10C rates. The capacity of the electrode can reach 158.6mAh / g at a rate of 0.2C, and even in the first cycle of the cycle at a large rate of 10C, it can reach a high capacity of 93.17mAh / g, and can maintain a capacity of 90.15mAh / g in the last cycle of 10C. After 70 cycles of rate cycling, the capacity retention rate is 96.8%.

[0065] Embodiment 2:

[0066] A method for preparing a reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric comprises the following steps:

[0067] (1) A graphene oxide dispersion with a concentration of 20 mg / mL was prepared, and the solvent was N,N-dimethylformamide (DMF), which was dispersion 1. The same dispersion with a concentration of 20 mg / mL was prepared, and dicyandiamide powder was added thereto and stirred thoroughly. The mass ratio of dicyandiamide to graphene oxide powder was 20:1, which was dispersion 2.

[0068] (2) 2 mL of dispersion 1 was injected into a rotating ethyl acetate coagulation bath using a needle with an inner diameter of 210 μm at an injection speed of 300 μL / min, the coagulation bath was rotated at 30 rpm, and the solution was allowed to stand for 2 h. 1 mL of dispersion 2 was injected into another rotating ethyl acetate coagulation bath using a needle with an inner diameter of 160 μm at an injection speed of 240 μL / min, the coagulation bath was rotated at 30 rpm, and the solution was allowed to stand for 2 h.

[0069] (3-5) Step 3-5 is the same as Example 1

[0070] The SEM scanning image of the obtained nonwoven fabric is as follows: Figure 7 As shown in (a): It can be seen that when the content of dicyandiamide powder is increased, the fusion effect between the fibers is weakened and the non-woven fabric structure becomes loose.

[0071] Embodiment 3:

[0072] (1) Step 1 is the same as Example 2

[0073] (2) 2 mL of dispersion 1 was injected into a rotating ethyl acetate coagulation bath using a needle with an inner diameter of 160 μm at an injection speed of 200 μL / min, the coagulation bath was rotated at 30 rpm, and the solution was allowed to stand for 1 h. 2 mL of dispersion 2 was injected into another rotating ethyl acetate coagulation bath using a needle with an inner diameter of 110 μm at an injection speed of 150 μL / min, the coagulation bath was rotated at 30 rpm, and the solution was allowed to stand for 1 h.

[0074] (3-4) Step 3-4 is the same as Example 1

[0075] (5) The non-woven fabric pieces are carbonized at a temperature of 600°C, a heating rate of 2°C / min, and a holding time of 2.5 h to obtain battery electrodes.

[0076] The SEM scanning image of the obtained nonwoven fabric is as follows Figure 7 (b) shows that when the amount of graphene oxide fibers is reduced, the fusion effect between the fibers is weakened, the non-woven fabric structure becomes loose, and the fibers become coarse.

[0077] Embodiment 4:

[0078] (1) A graphene oxide dispersion with a concentration of 10 mg / mL was prepared, and the solvent was N,N-dimethylformamide (DMF), which was dispersion 1. The same dispersion with a concentration of 10 mg / mL was prepared, and dicyandiamide powder was added thereto and stirred thoroughly. The mass ratio of dicyandiamide to graphene oxide powder was 15:1, which was dispersion 2.

[0079] (2) 3 mL of dispersion 1 was injected into a rotating ethyl acetate coagulation bath using a needle with an inner diameter of 160 μm at an injection speed of 80 μL / min, the coagulation bath rotation speed was 20 rpm, and the solution was allowed to stand for 2 h. 2 mL of dispersion 2 was injected into another rotating ethyl acetate coagulation bath using a needle with an inner diameter of 60 μm at an injection speed of 50 μL / min, the coagulation bath rotation speed was 20 rpm, and the solution was allowed to stand for 2 h.

[0080] (3-4) Step 3-4 is the same as Example 1

[0081] (5) The non-woven fabric pieces are carbonized at a temperature of 520°C, a heating rate of 3°C / min, and a holding time of 2 h to obtain battery electrodes.

[0082] The obtained nonwoven fabric was tested by XRD and XPS, and the detected N content and g-C3N4 content were extremely small. It can be seen that the control of heat treatment is also very important for the formation of g-C3N4. Generally, suitable temperature, low heating rate and longer insulation are required to form good g-C3N4.

[0083] Embodiment 5:

[0084] (1) Step 1 is the same as Example 1

[0085] (2) 2 mL of dispersion 1 was injected into a rotating ethyl acetate coagulation bath using a needle with an inner diameter of 260 μm at an injection rate of 450 μL / min, the coagulation bath was rotated at 40 rpm, and the solution was allowed to stand for 2 h. 1.5 mL of dispersion 2 was injected into another rotating ethyl acetate coagulation bath using a needle with an inner diameter of 160 μm at an injection rate of 300 μL / min, the coagulation bath was rotated at 40 rpm, and the solution was allowed to stand for 2 h.

[0086] (3-4) Step 3-4 is the same as Example 1

[0087] (5) The non-woven fabric pieces are carbonized at a temperature of 580°C, a heating rate of 2°C / min, and a holding time of 4 hours to obtain battery electrodes.

[0088] The obtained nonwoven fiber diameter is larger than that of Example 1. Therefore, when the inner diameter of the needle increases, the fiber diameter will also increase, and vice versa.

[0089] Embodiment 6:

[0090] (1) A graphene oxide raw material with higher oxidizability than that in Example 1 was selected to prepare each dispersion liquid. The remaining steps were the same as in Example 1. The experiment was carried out and the obtained sample was recorded as 6-1.

[0091] (2) The graphene oxide dispersion in step 1 was subjected to hydrothermal reduction and reacted in a hydrothermal reactor at a reaction temperature of 90° C. for 2 h to remove some oxygen-containing functional groups. The remaining steps were the same as those in Example 1. The obtained sample was recorded as 6-2.

[0092] The results showed that due to the poor mechanical properties of the spun fibers, sample 6-1 did not produce a non-woven fabric, indicating that raw materials with too high an oxygen content were difficult to spin and thus form a non-woven fabric; while sample 6-2 was a complete non-woven fabric, indicating that after reducing graphene oxide, the mechanical properties of the spun fibers could be enhanced, thus better forming a non-woven fabric.

[0093] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. Therefore, the scope of protection of the present invention should be subject to the scope of protection of the claims.

Claims

1. A method for preparing a reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric, characterized in that: The following steps are involved: S1. Using N,N-dimethylformamide as solvent, the monolayer graphene oxide powder is uniformly dispersed by using a cell crusher or ultrasound, and the concentration of the dispersion is 10-20 mg / mL to obtain a first dispersion, i.e., a monolayer graphene oxide dispersion; S2, preparing a monolayer graphene oxide dispersion with the same concentration using the same method as step S1, adding dicyandiamide powder to the treated dispersion, and stirring thoroughly to obtain a second dispersion; S3, using the first dispersion and the second dispersion to perform wet spinning respectively, to obtain reduced graphene oxide fibers and reduced graphene oxide / graphite-like carbon nitride fibers composited in a certain proportion and in a certain form; the spinning uses ethyl acetate as a coagulation bath; wherein the inner diameter of the needle for injecting the second dispersion is smaller than the inner diameter of the needle for injecting the first dispersion, so that the spinning diameter of the reduced graphene oxide / graphite-like carbon nitride composite fibers is smaller than the spinning diameter of the reduced graphene oxide fibers; S4, placing the spun fiber obtained in step S3 in a coagulation bath to perform solvent exchange; S5, filtering the mixture of step S4 on a Buchner funnel; S6, soaking the two types of fibers after filtration in an acetone solution added with saturated dicyandiamide, and performing solvent exchange again; S7, lightly stirring the mixture solution of step S6, and then filtering and collecting it with a filter screen, and the collected fibers are accumulated into a cake-like substance of a certain thickness; S8, putting the collected cakes into an oven for drying; S9, carbonizing the sample slide dried in step S8 in a tube furnace, and naturally cooling to room temperature after carbonization to obtain the reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric.

2. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: The step S1 comprises a centrifugal separation step: subjecting the dispersion formed by the cell crusher or ultrasonic dispersion to one to three differential centrifugations, with the centrifugal speed controlled at 6000-12000 rpm, taking the precipitate and then dispersing it with N,N-dimethylformamide.

3. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: In the step S2, the mass ratio of dicyandiamide to monolayer graphene oxide is: (10:1) to (20:1).

4. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: The specific operation of step S3 is as follows: the first dispersion liquid is injected into the ethyl acetate coagulation bath with a rotation speed of 20 to 40 rpm at an injection speed of 80 to 500 μL / min, and the second dispersion liquid is injected into the ethyl acetate coagulation bath at an injection speed of 50 to 300 μL / min.

5. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: In step S3, the inner diameter of the needle for injecting the first dispersion is 160 μm to 260 μm; the inner diameter of the needle for injecting the second dispersion is 60 μm to 160 μm; The ethyl acetate coagulation bath into which the second dispersion is injected is the same coagulation bath into which the first dispersion is injected or a separate coagulation bath having the same rotation speed as the ethyl acetate coagulation bath into which the first dispersion is injected.

6. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: In the step S4, the spun fiber is kept in the coagulation bath for 10 to 180 minutes; In step S6, the fiber is immersed in the acetone solution containing saturated dicyandiamide for 10 to 180 minutes.

7. The method for preparing the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric according to claim 1, characterized in that: In step S8, the drying temperature is 60-90°C; In step S9, the temperature mechanism of carbonization is as follows: the heating rate is 2-3°C / min, the carbonization temperature is 520-600°C, and the holding time is 2-4h.

8. A reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric prepared by the method for preparing a reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric as claimed in claim 1, characterized in that: The nonwoven fabric is a multilayer structure formed by overlapping reduced graphene oxide / graphite-like carbon nitride composite fibers and reduced graphene oxide fibers; the volume ratio of the reduced graphene oxide fibers to the reduced graphene oxide / graphite-like carbon nitride composite fibers is (2:1) to (1:1); and the diameter range of the fibers is 30-70 μm.

9. An application of the reduced graphene oxide / graphite-like carbon nitride composite nonwoven fabric as claimed in claim 8, characterized in that: The non-woven fabric is flexible and is used as a three-dimensional skeleton in the negative electrode of a lithium metal battery. The reduced graphene oxide / graphite-like carbon nitride composite non-woven fabric serves as a substrate for lithium metal deposition.