Purification method of crude pyromellitic dianhydride and preparation method of pyromellitic dianhydride
Through the sublimation purification method under negative pressure, the purification process of phthalic acid dianhydride is simplified, the product purity is improved, the problems of complex and low purity in the existing technology are solved, and the high purity of phthalic acid dianhydride is achieved Preparation of formic dianhydride.
Patent Information
- Application Number
- CN202111160482.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-30
AI Technical Summary
The existing phthalic acid dianhydride purification method is complex and the product is low in purity, making it difficult to meet the requirements of industrial polymerization grade.
Using the sublimation purification method under negative pressure, the crude phthalic acid dianhydride is heated in the sublimation chamber to sublimate it into vapor, and condensed in the sublimation finger to obtain the purified phthalic acid dianhydride, and sublimation-condensation operations are performed multiple times. Can improve purity.
It achieves simple process flow and easy operation. The purity of purified phthalic acid dianhydride can reach 99%, meeting the requirements of industrial polymerization grade.
Smart Images

Figure CN115894511B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic compound purification, and in particular to a method for purifying crude pyrophthalic acid dianhydride and a method for preparing pyrophthalic acid dianhydride. Background Art
[0002] Phenyltetracarboxylic dianhydride (MPDA) is an organic chemical intermediate. Thermoplastic polyimide (TPI) special engineering plastics produced with high-purity MPDA as raw material have a wide range of uses in electromechanical, electronic, aviation and other fields.
[0003] There are usually two methods for industrial production of phthalic anhydride: one is the gas phase oxidation method, where phthalic anhydride reacts chemically with oxygen in the air under the action of a catalyst to produce MPDA; the other is the liquid phase oxidation method, where phthalic anhydride is used as a raw material and nitric acid is used to liquid phase oxidize phthalic acid to produce phthalic acid, which is further dehydrated to produce MPDA. Whether it is the gas phase oxidation method or the liquid phase oxidation method, while the reaction produces MPDA, side reactions also occur to produce some partially oxidized or over-oxidized solid by-products, such as trimellitic acid or trimellitic anhydride (TMA). Since MPDA has a high melting point (198.5-205.5°C) and a high boiling point (492.8-558.8°C), the by-products also have the characteristics of high melting point and high boiling point. In the process of recovering MPDA, crude anhydrides with different impurity (by-product) contents are often obtained. Therefore, the purification process of the by-products and the anhydrides in the crude anhydride is a key link in the production of MPDA.
[0004] The existing methods for refining phenyltetracarboxylic anhydride mainly include distillation, solvent and high-temperature gas carrying. The distillation method is to use the different boiling points of the distillation raw materials to extract different fractions from the top or middle of the distillation tower, but this method has strict requirements on the purity and boiling point of the raw materials, and the purity of the raw materials generally needs to be greater than 95%; the solvent method is to use the solubility of different substances in the solvent to purify the substance. If you want to obtain a high-purity extract, you need to refine the product multiple times, but the loss of the product will also increase accordingly; and the high-temperature gas carrying method is to use the characteristics of product sublimation to use high-temperature gas to sublimate the product, and then cool the mixed gas to condense the product. If large-scale production is required, a large amount of gas must be used for carrying, and gas heating and cooling also require large equipment, especially for cooling equipment. If the cooling equipment is small, the mixed gas flow rate will be too fast, which will cause the condensed fine particles to not settle down, increasing the loss of the purified product. Summary of the invention
[0005] The invention aims to overcome the problems in the prior art that the refining method of crude phenyltetracarboxylic dianhydride is complicated and the purity of the obtained product is low, and to provide a method for purifying crude phenyltetracarboxylic dianhydride; the purification method has a short process flow, is simple to operate, and the purified phenyltetracarboxylic dianhydride has high purity and can meet the requirements of industrial polymerization grade.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for purifying phenyltetracarboxylic dianhydride, which comprises: subliming crude phenyltetracarboxylic dianhydride under negative pressure to obtain phenyltetracarboxylic dianhydride vapor, and condensing the vapor to obtain purified phenyltetracarboxylic dianhydride.
[0007] Preferably, the purification method is carried out in a sublimation purification device, which comprises: a sublimation chamber, a sublimation finger;
[0008] A sublimation chamber, used to contain crude phthalic acid anhydride, capable of heating to sublimate the crude phthalic acid anhydride into vapor, and the sublimation chamber can be maintained in a negative pressure state by an external vacuum pumping device;
[0009] Sublimation refers to the process of condensing the vapor of phthalic anhydride in the sublimation chamber;
[0010] The purification method comprises:
[0011] Under negative pressure, the sublimation chamber is heated to sublimate the crude dianhydride to obtain dianhydride vapor, and the vapor is condensed in the sublimation finger to obtain purified dianhydride.
[0012] According to a second aspect of the present invention, the present invention provides a method for preparing pyromellitic dianhydride, the method comprising:
[0013] 1) adding phenyltetracarboxylic acid to the second acid anhydride to obtain a solution, and heating the solution;
[0014] 2) after the solution is cooled to room temperature, a poor solvent is added to precipitate a solid, and after solid-liquid separation, the solid is dried to prepare crude phenyltetracarboxylic dianhydride;
[0015] 3) Purify the crude phthalic acid anhydride according to the above purification method.
[0016] The method for purifying pyrophthalic acid dianhydride provided by the present invention utilizes the sublimation points of different acid anhydrides to purify pyrophthalic acid dianhydride by sublimation-desublimation of pyrophthalic acid dianhydride under negative pressure, and multiple purifications can improve the purity of pyrophthalic acid dianhydride. The method of the present invention is preferably carried out in the sublimation purification device of the present invention, the sublimation purification device has a simple structure, the purification method has a short process flow, and the operation is simple. The purified pyrophthalic acid dianhydride has high purity and can meet the requirements of industrial polymerization grade.
[0017] The preparation method of phthalic acid dianhydride of the present invention, the crude phthalic acid dianhydride prepared by the method is particularly suitable for purification by the purification method of the present application, and the purity of the purified phthalic acid dianhydride can be as high as 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The invention discloses a sublimation purification device provided in a preferred embodiment of the present invention.
[0019] Description of Reference Numerals
[0020] 1—Sublimation chamber
[0021] 2—Sublimation
[0022] 3—First cooling medium circulation interface
[0023] 4—Second cooling medium circulation interface
[0024] 5—Vacuum extraction interface
[0025] 6—First valve DETAILED DESCRIPTION
[0026] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0027] The structural formula of pyromellitic dianhydride is shown in structural formula (I); the structural formula of pyromellitic acid (MPA) is shown in structural formula (II):
[0028]
[0029] According to a first aspect of the present invention, the present invention provides a method for purifying pyromellitic dianhydride, the purification method comprising:
[0030] Under negative pressure, crude pyrophthalic acid anhydride is sublimated to obtain pyrophthalic acid anhydride vapor, and the vapor is condensed to obtain purified pyrophthalic acid anhydride. The present invention utilizes the sublimation points of different acid anhydrides to purify pyrophthalic acid anhydride by sublimation-condensation of pyrophthalic acid anhydride under negative pressure. The prior art hydrolyzes crude pyrophthalic acid anhydride to obtain pyrophthalic acid and then dehydrates it into anhydride for purification. Compared with the purification method of the prior art, the present invention has the advantages of simple process, high yield and high product purity.
[0031] According to a preferred embodiment of the present invention, the sublimation conditions include: a sublimation temperature of 150-250° C.; under such sublimation conditions, the purity of phenyltetracarboxylic dianhydride is improved.
[0032] In the present invention, the sublimation time is determined according to the temperature. According to a preferred embodiment of the present invention, the sublimation conditions include: the sublimation time is 1 to 20 hours; under the sublimation conditions, the purity of phthalic acid dianhydride is improved.
[0033] According to the present invention, the conditions for desublimation include: the condensation temperature is -10°C to 20°C.
[0034] In the present invention, the vacuum degree can be selected in a wide range, as long as it can make phthalic acid dianhydride sublime. According to a preferred embodiment of the present invention, the sublimation conditions include: the vacuum degree is 0.01-0.05 kPa; under such sublimation conditions, the purity of phthalic acid dianhydride is improved.
[0035] The object of the present invention can be achieved by the above-mentioned method of the present invention, and there is no special requirement for the equipment used. According to a preferred embodiment of the present invention, the purification method is carried out in a sublimation purification device, and the sublimation purification device comprises: a sublimation chamber, a sublimation finger;
[0036] A sublimation chamber, used to contain crude phthalic acid anhydride, capable of heating to sublimate the crude phthalic acid anhydride into vapor, and the sublimation chamber can be maintained in a negative pressure state by an external vacuum pumping device;
[0037] Sublimation refers to the process of condensing the vapor of phthalic anhydride in the sublimation chamber;
[0038] The purification method comprises:
[0039] Under negative pressure, the sublimation chamber is heated to sublimate crude phthalic anhydride to obtain phthalic anhydride vapor, and the vapor is condensed in the sublimation finger to obtain purified phthalic anhydride, which is beneficial to improve the purity of phthalic anhydride.
[0040] According to a preferred embodiment of the present invention, the purification method is carried out in a sublimation purification device, and the sublimation conditions include: a sublimation temperature of 150 to 250° C.; under the sublimation conditions, the purity of phthalic acid dianhydride is improved.
[0041] According to a preferred embodiment of the present invention, the purification method is carried out in a sublimation purification device, and the sublimation conditions include: a sublimation time of 1 to 20 hours; under the sublimation conditions, it is beneficial to improve the purity of phthalic acid dianhydride.
[0042] According to a preferred embodiment of the present invention, the purification method is carried out in a sublimation purification device, and the sublimation conditions include: a vacuum degree of 0.01 to 0.05 kPa; under the sublimation conditions, the purity of phenyltetracarboxylic dianhydride is improved.
[0043] According to a preferred embodiment of the present invention, the purification method is carried out in a sublimation purification device, and the sublimation conditions include: the sublimation refers to a condensation temperature of -10-20°C; under the sublimation conditions, it is beneficial to improve the purity of phthalic acid dianhydride.
[0044] According to a preferred embodiment of the present invention, the sublimation-desublimation operation is repeated 2-5 times; preferably, the sublimation time of the latter sublimation is greater than the sublimation time of the previous sublimation. For example, the second sublimation-desublimation-desublimation time is greater than the first sublimation-desublimation time; for example, the sublimation time of the second and third purifications is 10 to 50 hours; this is beneficial to improving the purity of phenyltetracarboxylic dianhydride.
[0045] According to a preferred embodiment of the present invention, the sublimation purification device is as follows Figure 1 As shown, the sublimation purification device includes: a sublimation chamber 1, a sublimation finger 2, a vacuum interface 5, and a first valve 6;
[0046] The sublimation chamber 1 is used to contain crude phthalic anhydride and can be heated to sublime the crude phthalic anhydride into vapor, and the sublimation chamber 1 can maintain a negative pressure state with an external vacuum device through a vacuum interface 5; the first valve 6 is used to control the vacuum degree;
[0047] The sublimation finger 2 is arranged in the sublimation chamber 1 for condensing the vapor of phthalic acid dianhydride; the sublimation finger 2 comprises a first cooling medium circulation interface 3 and a second cooling medium circulation interface 4, and the cooling medium enters the sublimation finger 2 from the first cooling medium circulation interface 3 for refrigeration and flows out from the second cooling medium circulation interface 4.
[0048] According to a preferred embodiment of the present invention, the purification method comprises:
[0049] The sublimation chamber 1 is placed in a negative pressure state by means of the vacuum interface 5 , and the sublimation chamber 1 is heated to sublime the crude phthalic anhydride to obtain phthalic anhydride vapor, and the vapor is condensed in the sublimation finger 2 to obtain purified phthalic anhydride.
[0050] According to the present invention, while pyrophthalic acid reacts to generate pyrophthalic anhydride, a side reaction also occurs to generate some partially oxidized or over-oxidized solid by-products, such as trimellitic acid or trimellitic anhydride (TMA). According to a preferred embodiment of the present invention, the purity of the crude pyrophthalic anhydride used for purification is ≥80.1%, which is beneficial to improve the purity of pyrophthalic anhydride while reducing power consumption.
[0051] According to a preferred embodiment of the present invention, the sublimation-desublimation operation times and conditions are controlled so that the purity of the purified phenyltetracarboxylic dianhydride is ≥85%; more preferably, the purity is ≥96%; and more preferably, the purity is ≥98%.
[0052] According to a second aspect of the present invention, the present invention provides a method for preparing pyromellitic dianhydride, the method comprising:
[0053] 1) adding phenyltetracarboxylic acid to the second acid anhydride to obtain a solution, and heating the solution;
[0054] 2) after the solution is cooled to room temperature, a poor solvent is added to precipitate a solid, and after solid-liquid separation, the solid is dried to prepare crude phenyltetracarboxylic dianhydride;
[0055] 3) Purifying the crude pyrophthalic acid anhydride according to the aforementioned purification method. The aforementioned preparation method of pyrophthalic acid anhydride is beneficial to improving the purity of pyrophthalic acid anhydride while reducing power consumption.
[0056] In the present invention, the second acid anhydride has a wide range of optional types and is mainly used as a dehydrating agent. According to a preferred embodiment of the present invention, the second acid anhydride is selected from one or more of acetic anhydride, BOC anhydride and propionic anhydride.
[0057] In the present invention, the poor solvent can be selected from a wide range of types. For the present invention, the poor solvent is preferably selected from one or more of ether, petroleum ether, ethyl acetate and isopropyl ether. The preparation method of the crude pyrophthalic acid dianhydride of the present invention, combined with the purification method of the crude pyrophthalic acid provided by the present invention, is conducive to further improving the purity of pyrophthalic acid dianhydride.
[0058] According to the present invention, the mass ratio of pyromellitic acid to the second acid anhydride can be selected in a wide range, and commonly used mass ratios can be used in the present invention. For the present invention, preferably, in step 1), the mass ratio of pyromellitic acid to the second acid anhydride is 1:5-10, preferably 1:7-9; which is beneficial to further improve the purity of pyromellitic dianhydride.
[0059] According to the present invention, in step 1), heating is mainly used for dehydration. Preferably, in step 1), the heating temperature is 140-180° C., preferably 150-170° C.; at this temperature, boiling and reflux are beneficial to further improve the purity of phthalic acid dianhydride.
[0060] According to the present invention, in step 1), the heating time is determined according to the temperature. For the present invention, preferably, in step 1), the heating time is 1-5h, preferably 2-4h; reasonably adjusting the heating time by the heating temperature is conducive to further improving the purity of phthalic acid dianhydride.
[0061] According to the present invention, in step 2), the mass content of phenyltetracarboxylic dianhydride in the cooled solution is 50-80wt%, which is beneficial to further improve the purity and yield of phenyltetracarboxylic dianhydride.
[0062] According to the present invention, in step 2), phthalic acid dianhydride is precipitated by a poor solvent, and the mass ratio of the second acid anhydride to the poor solvent is 1:2-5; this is beneficial to further improve the purity and yield of phthalic acid dianhydride.
[0063] The present invention has no particular limitation on the drying method of the crude phthalic anhydride product obtained by solid-liquid separation. Optionally, the drying method may be blast drying or vacuum drying. In order to further improve the purity of phthalic anhydride, preferably, the drying method is vacuum drying. More preferably, the vacuum drying conditions include: a drying temperature of 50-90° C.; and a vacuum degree of 0.01-0.05 kPa.
[0064] The present invention will be described in detail below through examples.
[0065] Example 1
[0066] 1) Add phenyltetracarboxylic acid (5 g) to acetic anhydride (35 g), heat to boil at 150°C, keep reflux, the mixture gradually turns black during boiling, and finally forms a black solution;
[0067] 2) After the solution is cooled, ether (70 g) is added to precipitate solid phthalic anhydride, which is then filtered and dried in a vacuum oven at 70° C. to obtain crude phthalic anhydride;
[0068] 3) The crude benzoic anhydride is placed in a sublimation chamber 1, the sublimation temperature is 190° C., the sublimation time is 5 hours, and the vacuum is continuously drawn during the sublimation process and the vacuum degree is maintained at 0.05 kPa. The temperature of the coolant passing through the sublimation finger 2 is 20° C.; after the sublimation-desublimation operation is completed, the crystal on the sublimation finger 2 is removed and placed in the sublimation chamber for the second sublimation-desublimation and the third sublimation-desublimation. The sublimation temperature is 190° C., the sublimation time is 10 hours, and the vacuum is continuously drawn during the sublimation process and the vacuum degree is maintained at 0.05 kPa.
[0069] After the third sublimation-desublimation purification, a light yellow solid is obtained. The purity of the phenyltetracarboxylic dianhydride purified by the three sublimation-desublimation purifications is 85.5%, 95% and 98% respectively, which can meet the requirements of industrial polymerization grade.
[0070] Example 2
[0071] 1) Add phenyltetracarboxylic acid (5 g) to acetic anhydride (45 g), heat to boil at 170°C, keep reflux, and the mixture gradually turns black during boiling to form a black solution;
[0072] 2) After the solution is cooled, ether (180 g) is added to precipitate solid phthalic anhydride, which is then filtered and dried in a vacuum oven at 70° C. to obtain crude phthalic anhydride;
[0073] 3) crude benzoic acid anhydride is placed in a sublimation chamber 1, the sublimation temperature is 220°C, the sublimation time is 8 hours, and the vacuum is continuously drawn during the sublimation process to maintain a vacuum degree of 0.05 kPa. The temperature of the coolant passing through the sublimation finger 2 is -10°C; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for a second sublimation-desublimation and a third sublimation-desublimation-desublimation. The sublimation temperature is 195°C, the sublimation time is 16 hours, and the vacuum is continuously drawn during the sublimation process to maintain a vacuum degree of 0.05 kPa.
[0074] After the third sublimation-desublimation purification, a light yellow solid is obtained. The purity of the phenyltetracarboxylic dianhydride after the three sublimation-desublimation is 86%, 95% and 98.2% respectively, which can meet the requirements of industrial polymerization grade.
[0075] Example 3
[0076] 1) Add phenyltetracarboxylic acid (5 g) to acetic anhydride (40 g), heat to boil at 160°C, keep reflux, and the mixture gradually turns black during boiling to form a black solution;
[0077] 2) After the solution is cooled, ether (120 g) is added to precipitate solid phthalic acid anhydride, which is then filtered and dried in a vacuum oven at 90° C. to obtain crude phthalic acid anhydride;
[0078] 3) The crude benzoic anhydride is placed in a sublimation chamber 1, the sublimation temperature is 210° C., the sublimation time is 10 hours, and the vacuum is continuously drawn during the sublimation process to maintain a vacuum degree of 0.05 kPa. The temperature of the coolant passing through the sublimation finger 2 is 5° C.; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for a second sublimation-condensation and a third sublimation-condensation. The sublimation temperature is 210° C., the sublimation time is 20 hours, and the vacuum is continuously drawn during the sublimation process to maintain a vacuum degree of 0.05 kPa.
[0079] After the third sublimation-desublimation-desublimation purification, a light yellow solid is obtained. The purity of the phenyltetracarboxylic dianhydride after the three sublimation-desublimation is 88%, 96% and 99% respectively, which can meet the requirements of industrial polymerization grade.
[0080] Example 4
[0081] 1) Add 5 g of benzoic acid to 60 g of acetic anhydride, heat to boil at 130°C, and keep reflux. During the boiling process, the mixture gradually turns black and finally forms a black solution;
[0082] 2) After the solution is cooled, ether (100 g) is added to precipitate solid phthalic anhydride, which is then filtered and dried in a vacuum oven at 90° C. to obtain crude phthalic anhydride;
[0083] 3) The crude benzoic anhydride is placed in a sublimation chamber 1, the sublimation temperature is 200°C, the sublimation time is 10 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa. The temperature of the coolant passing through the sublimation finger 2 is 0°C; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for the second sublimation-condensation and the third sublimation-condensation. The sublimation temperature is 200°C, the sublimation time is 15 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa.
[0084] After the third sublimation-desublimation-desublimation purification, a light yellow solid is obtained. The purity of the phenyltetracarboxylic dianhydride after the three sublimation-desublimation is 85%, 96.3% and 96.9% respectively, which can meet the requirements of industrial polymerization grade.
[0085] Example 5
[0086] 1) Add 5 g of benzoic acid to 60 g of acetic anhydride, heat to boil at 130°C, and keep reflux. During the boiling process, the mixture gradually turns black and finally forms a black solution;
[0087] 2) After the solution is cooled, ether (50 g) is added to precipitate solid phthalic acid anhydride, which is then filtered and dried in a vacuum oven at 90° C. to obtain crude phthalic acid anhydride;
[0088] 3) The crude benzoic anhydride is placed in a sublimation chamber 1, the sublimation temperature is 200°C, the sublimation time is 10 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa. The temperature of the coolant passing through the sublimation finger 2 is 0°C; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for the second sublimation-condensation and the third sublimation-condensation. The sublimation temperature is 200°C, the sublimation time is 15 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa.
[0089] After the third sublimation-desublimation-desublimation purification, a light yellow solid is obtained. The purity of the phenyltetracarboxylic dianhydride after the three sublimation-desublimation is 82%, 90% and 95% respectively.
[0090] Example 6
[0091] 1) Add benzoic acid (5 g) to acetic anhydride (25 g), heat at 130°C, keep reflux, and the mixture gradually turns black during boiling to form a black solution;
[0092] 2) After the solution is cooled, ether (100 g) is added to precipitate solid phthalic anhydride, which is then filtered and dried in a vacuum oven at 90° C. to obtain crude phthalic anhydride;
[0093] 3) The crude benzoic anhydride is placed in a sublimation chamber 1, the sublimation temperature is 200°C, the sublimation time is 10 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa. The temperature of the coolant passing through the sublimation finger 2 is 0°C; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for the second sublimation-condensation and the third sublimation-condensation. The sublimation temperature is 200°C, the sublimation time is 15 hours, and the vacuum is continuously drawn during the sublimation process to maintain the vacuum degree at 0.03 kPa.
[0094] After the third sublimation-desublimation-desublimation purification, a light yellow solid was obtained. The purity of the phenyltetracarboxylic dianhydride after the three sublimation-desublimation was 76%, 88% and 92% respectively.
[0095] Comparative Example 1
[0096] 1) Add 5 g of benzoic acid to 60 g of acetic anhydride, heat to boil at 130°C, and keep reflux. During the boiling process, the mixture gradually turns black and finally forms a black solution;
[0097] 2) After the solution is cooled, ether (100 g) is added to precipitate solid phthalic anhydride, which is then filtered and dried in a vacuum oven at 90° C. to obtain crude phthalic anhydride;
[0098] 3) Crude phenyltetracarboxylic dianhydride is placed in a sublimation chamber 1, the sublimation temperature is 200°C, the sublimation time is 10 hours, and the sublimation is carried out under normal pressure. The temperature of the coolant passing through the sublimation finger 2 is 0°C; after the sublimation is completed, the crystals on the sublimation finger 2 are removed and placed in a sublimator for the second sublimation-condensation and the third sublimation-condensation. The sublimation temperature is 200°C, the sublimation time is 15 hours, and the sublimation is carried out under normal pressure.
[0099] After the third purification, a light yellow solid was obtained. The purity of the phthalic acid dianhydride after the three purifications was 73%, 85% and 87% respectively.
[0100] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing pyromellitic dianhydride, characterized in that: The method includes: 1) adding phenyltetracarboxylic acid to the second acid anhydride to obtain a solution, and heating the solution at a temperature of 140-180° C.; 2) after the solution is cooled to room temperature, a poor solvent is added to precipitate a solid, and after solid-liquid separation, the solid is dried to prepare crude phenyltetracarboxylic dianhydride; 3) Purifying the crude phthalic acid anhydride according to the following purification method; Under negative pressure, crude phthalic acid anhydride is sublimated to obtain phthalic acid anhydride vapor, and the vapor is condensed to obtain purified phthalic acid anhydride; The second anhydride is selected from one or more of acetic anhydride, BOC anhydride and propionic anhydride; The poor solvent is selected from one or more of diethyl ether, petroleum ether, ethyl acetate and isopropyl ether.
2. The preparation method according to claim 1, wherein Sublimation conditions include: Sublimation temperature is 150-250°C; and / or Sublimation time is 1 to 20 hours; and / or The vacuum degree is 0.01-0.05 kPa; and / or The conditions for condensation include: condensation temperature is -10℃~20℃; The purity of the crude phthalic acid dianhydride used for purification is ≥80.1%.
3. The preparation method according to claim 1, wherein In step 3), the purification method is carried out in a sublimation purification device, and the sublimation purification device includes: a sublimation chamber, a sublimation finger; A sublimation chamber, used to contain crude phthalic acid anhydride, capable of heating to sublimate the crude phthalic acid anhydride into vapor, and the sublimation chamber can be maintained in a negative pressure state by an external vacuum pumping device; Sublimation refers to the process of condensing the vapor of phthalic anhydride in the sublimation chamber; The purification method comprises: Under negative pressure, the sublimation chamber is heated to sublimate the crude phthalic anhydride to obtain phthalic anhydride vapor, and the vapor is condensed in the sublimation finger to obtain purified phthalic anhydride.
4. The preparation method according to claim 3, wherein The sublimation purification device comprises: a sublimation chamber (1), a sublimation finger (2), a vacuum extraction interface (5), a first valve 6, a first cooling medium circulation interface (3), and a second cooling medium circulation interface (4); The sublimation chamber (1) is used to contain crude phthalic acid anhydride and can be heated to sublime the crude phthalic acid anhydride into vapor, and the sublimation chamber (1) can maintain a negative pressure state with an external vacuum device through a vacuum interface (5); the first valve (6) is used to control the vacuum degree of the vacuum interface (5); The sublimation finger (2) is arranged in the sublimation chamber (1) and is used for condensing the vapor of phthalic acid anhydride; the sublimation finger (2) comprises the first cooling medium circulation interface (3) and the second cooling medium circulation interface (4); the cooling medium enters the sublimation finger (2) from the first cooling medium circulation interface (3) for refrigeration and flows out from the second cooling medium circulation interface (4); The purification method comprises: The sublimation chamber (1) is placed in a negative pressure state by means of a vacuum interface (5), and the sublimation chamber (1) is heated to sublime the crude phthalic anhydride to obtain phthalic anhydride vapor, and the vapor is condensed through a sublimation finger (2) to obtain purified phthalic anhydride.
5. The preparation method according to claim 4, wherein Sublimation conditions include: Sublimation temperature is 150-250°C; and / or Sublimation time is 1 to 20 hours; and / or The vacuum degree is 0.01~0.05kPa.
6. The preparation method according to claim 3 or 4, wherein: Sublimation refers to the condensation temperature of -10℃~20℃.
7. The preparation method according to claim 1 or 2, wherein: Repeat the sublimation-desublimation operation 2-5 times.
8. The preparation method according to claim 7, wherein: The latter sublimation time is greater than the previous sublimation time.
9. The preparation method according to claim 1 or 2, wherein: The sublimation-desublimation operation times and conditions are controlled so that the purity of the purified phenyltetracarboxylic dianhydride is ≥85%.
10. The preparation method according to claim 1 or 2, wherein: The sublimation-desublimation operation times and conditions are controlled so that the purity of the purified phenyltetracarboxylic dianhydride is ≥96%.
11. The preparation method according to claim 1 or 2, wherein: The sublimation-desublimation operation times and conditions are controlled so that the purity of the purified phenyltetracarboxylic dianhydride is ≥98%.
12. The preparation method according to claim 1, wherein: In step 1), the mass ratio of pyromellitic acid to the second acid anhydride is 1:5-10; and / or The heating time is 1-5h; and / or In step 2), the mass content of phthalic anhydride in the cooled solution is 50-80wt%; and / or The mass ratio of the second acid anhydride to the poor solvent is 1:2-5.
13. The preparation method according to claim 1, wherein The drying method is vacuum drying; the vacuum drying conditions include: the drying temperature is 50-90°C; The vacuum degree is 0.01-0.05kPa.