A tannic acid-modified protein-based hydrogel and its preparation method and application

By introducing tannic acid and calcium ions into the protein/sodium alginate hydrogel to form a cross-linked structure, the problem of insufficient tensile strength of traditional hydrogels is solved, and a hydrogel with high tensile strength and multifunctional properties is obtained. Glue, suitable for biomedical materials.

CN115895281BActive Publication Date: 2024-10-01TAIYUAN UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211503955.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-10-01
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Traditional natural polymer hydrogels are easy to break under external stimulation and have a single function, which limits their application in the biomedical field. In particular, protein hydrogels have low tensile strength and are difficult to meet the needs of tissue engineering and wound dressings. .

Method used

Through glutamine transferase/calcium ion cross-linking protein/sodium alginate, and introducing tannic acid into the composite hydrogel system, a tannic acid-modified protein/sodium alginate hydrogel is formed using the soaking method to improve Its tensile strength and biocompatibility.

Benefits of technology

The obtained hydrogel has high tensile strength, water retention, antifreeze and antioxidant properties, and is suitable for tissue engineering scaffolds and skin dressings, significantly improving its application potential in the biomedical field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115895281B_ABST
    Figure CN115895281B_ABST
Patent Text Reader

Abstract

The present invention relates to a tannic acid-modified protein-based hydrogel and a preparation method and application thereof, belonging to the field of hydrogel materials, and solving the technical problem that the mechanical properties of protein-based natural polymer hydrogels are poor. The preparation method of the present invention comprises the following steps: (1) cross-linking gelatin / sodium alginate solution by glutaminase to obtain gelatin / sodium alginate pre-hydrogel; (2) treating the pre-hydrogel with calcium chloride solution for 1 min, and then rinsing with deionized water; (3) then soaking the hydrogel in tannic acid solution for 24 h, and then soaking it in calcium chloride solution for 1.5 h, to obtain tannic acid-modified gelatin / sodium alginate hydrogel. The hydrogel prepared by the present invention has better tensile properties; high swelling rate; water retention and antifreeze properties; strong antioxidant properties; good blood compatibility and cell compatibility. The hydrogel can be applied to tissue engineering scaffolds, skin dressings, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogels, and particularly relates to a tannic acid-modified protein-based hydrogel and a preparation method and application thereof. Background Art

[0002] Natural polymer hydrogels have similar physical and chemical properties to living tissues, good biocompatibility and biodegradability, and have become an important type of biomaterial in the biomedical field. However, traditional natural polymer hydrogels have weak mechanical properties, are prone to breakage under external stimulation, and have a single function, which seriously limits their application.

[0003] Gelatin, collagen, and casein are a class of natural biomacromolecules with good biocompatibility. The RGD sequence (arginine-glycine-aspartic acid) in proteins is conducive to cell adhesion, making them ideal for tissue engineering, wound dressings, and surgical adhesives. Proteins have been widely studied and expected to be used in the field of biomedical materials, but most single protein hydrogels are brittle, fragile, and easily degraded, which greatly limits their application. Currently, scientists have adopted a variety of methods to improve the mechanical strength of hydrogels, including double or multi-network hydrogels, nanocomposite hydrogels, and double cross-linked hydrogels.

[0004] Sodium alginate is a natural polysaccharide material extracted from seaweed. Its solution has high viscosity and can form an "eggshell" structure with calcium ions. The researchers introduced sodium alginate into the protein hydrogel system to improve the mechanical properties of the single hydrogel through the double network structure, but the tensile strength of the composite hydrogel is still very low.

[0005] Tannic acid is a polyphenol compound extracted from plants, containing a large number of phenolic hydroxyl groups. Tannic acid can cross-link proteins through hydrogen bonds and hydrophobic interactions, thereby increasing the tensile strength of protein-based hydrogels. However, when the concentration of tannic acid is high, precipitation is easily generated due to the strong hydrogen bonding between tannic acid and protein, and a uniform hydrogel cannot be formed. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a tannic acid-modified protein-based hydrogel and a preparation method and application thereof. Tannic acid is introduced into a composite hydrogel system by immersion method through glutaminase / calcium ion cross-linking protein / sodium alginate, so as to obtain a tannic acid-modified protein / sodium alginate hydrogel with certain mechanical strength, water retention, antifreeze and antioxidant properties, thereby improving the tensile strength of the protein-based hydrogel.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:

[0008] A method for preparing a tannic acid-modified protein-based hydrogel comprises the following steps:

[0009] S1, sodium alginate powder is dissolved in a mixed solution of deionized water and glycerol, and stirred evenly at 70°C to obtain a mixed solution A for use in the following step;

[0010] S2. The protein material is dissolved in deionized water and stirred evenly at 50°C to obtain a mixed solution B for later use;

[0011] S3, glutaminase was dissolved in deionized water, and stirred evenly at room temperature to obtain a mixed solution C for use in the next step;

[0012] S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D;

[0013] S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E;

[0014] S6. First, remove the bubbles in the mixed solution E prepared in step S5 by ultrasound; second, pour the mixed solution E into a mold and keep it warm at 45°C for 4 hours to form a protein / sodium alginate hydrogel; third, soak the protein / sodium alginate hydrogel in a calcium ion solution for 1 minute and then rinse with deionized water; finally, soak the protein / sodium alginate hydrogel in a tannic acid solution for 24 hours and then in a calcium ion solution for 1.5 hours to obtain a tannic acid-modified protein / sodium alginate hydrogel.

[0015] Furthermore, in the mixed solution A prepared in step S1, the concentration of sodium alginate is 1.0% wt / v-2.0% wt / v.

[0016] Furthermore, in the mixed solution B prepared in step S2, the concentration of the protein material is 10%-15% wt / v.

[0017] Furthermore, the protein material is one or more of gelatin, collagen or casein.

[0018] Furthermore, in the mixed solution C prepared in step S2, the concentration of transglutaminase is 0.8%-1.2% wt / v.

[0019] Furthermore, the solvents of the calcium ion solution and the tannic acid solution in step S6 are both a mixture of glycerol and deionized water.

[0020] Furthermore, the material of the mold in step S6 is plastic, which is more conducive to the molding and demoulding of the hydrogel.

[0021] A tannic acid-modified protein-based hydrogel prepared by the above method is used in tissue engineering scaffolds or skin dressings.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The protein / sodium alginate hydrogel prepared by the process steps provided by the present invention has high tensile strength, water retention, antifreeze, antioxidation and other properties, and good biocompatibility. This natural hydrogel with excellent performance is more practical and can be applied to tissue engineering scaffolds, skin dressings and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The macroscopic images of the hydrogels prepared in Example 1 and Comparative Example 1;

[0025] Figure 2 The tensile properties of the hydrogels prepared in Examples 1-3 are: a) elastic modulus, b) elongation at break;

[0026] Figure 3 The tensile properties of the hydrogels prepared in Examples 1, 2, 4, and 5 are: a) elastic modulus, b) elongation at break;

[0027] Figure 4 Tensile properties of the hydrogel prepared in Example 6: a) elastic modulus, b) elongation at break;

[0028] Figure 5 TA prepared in Example 6 0 / 0 and TA 0.3 / 0.4 a) Schematic diagram of stretching of hydrogel, b) schematic diagram of twisting, knotting, and stretching after knotting, and c) schematic diagram of lifting a 500g weight;

[0029] Figure 6 The hydrogel prepared in Example 6 was placed in an oven at 25°C and 10% relative humidity, and the mass of the hydrogel was measured at regular intervals and its a) water retention rate was calculated. On the sixth day, the hydrogel was bent with tweezers and photographed to record its b) morphology.

[0030] Figure 7 TA prepared in Example 6 0 / 0 and TA 0.3 / 0.4a) Comparison of tensile stress-strain curves of the hydrogel in the initial state and after being placed in a -20°C refrigerator for 1 day, and b) comparison of flexibility. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0032] The concepts mentioned in the following description are represented by their corresponding abbreviations:

[0033] Sodium alginate (SA), gelatin (G), transglutaminase (mTG), calcium ion (Ca 2+ ), tannic acid (TA).

[0034] Ca 2+ c Solution: c represents Ca 2+ The CaCl2 content in the solution is c, in w / v; the volume ratio of glycerol to water is 1:4.

[0035] TA a / b Solution: a means the TA content in the TA solution is a, in w / v; b means the glycerol content in the TA solution is b, in v / v.

[0036] Example 1

[0037] A method for preparing a tannic acid-modified protein-based hydrogel comprises the following steps:

[0038] S1. Weigh 1.5 g of SA powder and dissolve it in a mixed solution of 20 mL of deionized water and 20 mL of glycerol, and stir evenly at 70°C to obtain a mixed solution A for use in the next step;

[0039] S2, weigh 10 g of G particles and dissolve them in 40 mL of deionized water, and stir them evenly at 50°C to obtain a mixed solution B for use in the next step;

[0040] S3, weigh 0.8 g of mTG powder and dissolve it in 20 mL of deionized water, and stir it evenly at room temperature to obtain a mixed solution C for use in the next step;

[0041] S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D;

[0042] S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E;

[0043] S6. First, remove the bubbles in the mixed solution E prepared in step S5 by ultrasound; second, pour the mixed solution E into a mold made of plastic and keep it at 45°C for 4 hours to form a G / SA hydrogel; third, place the G / SA hydrogel in Ca 2+ 0.03 The G / SA hydrogel was immersed in TA 0.1 / 0.2 The tannic acid-modified protein / sodium alginate hydrogel (G / SA-TA hydrogel) was prepared by immersing the tannic acid-modified protein / sodium alginate hydrogel in the solution for 24 h. 2+ 0.03 Solution and TA 0.1 / 0.2 The solvent of the solution was a mixture of glycerol and deionized water.

[0044] The tannic acid-modified protein-based hydrogel prepared by the above method can be applied to tissue engineering scaffolds or skin dressings.

[0045] Example 2

[0046] A method for preparing a tannic acid-modified protein-based hydrogel comprises the following steps:

[0047] S1. Weigh 1.5 g of SA powder and dissolve it in a mixed solution of 20 mL of deionized water and 20 mL of glycerol, and stir evenly at 70°C to obtain a mixed solution A for use in the next step;

[0048] S2, weigh 10 g of G particles and dissolve them in 40 mL of deionized water, and stir them evenly at 50°C to obtain a mixed solution B for use in the next step;

[0049] S3, weigh 0.8 g of mTG powder and dissolve it in 20 mL of deionized water, and stir it evenly at room temperature to obtain a mixed solution C for use in the next step;

[0050] S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D;

[0051] S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E;

[0052] S6. First, remove the bubbles in the mixed solution E prepared in step S5 by ultrasound; second, pour the mixed solution E into a mold made of plastic and keep it at 45°C for 4 hours to form a G / SA hydrogel; third, place the G / SA hydrogel in Ca 2+ 0.03 The G / SA hydrogel was immersed in TA 0.3 / 0.2 The tannic acid-modified protein / sodium alginate hydrogel (G / SA-TA hydrogel) was prepared by immersing the tannic acid-modified protein / sodium alginate hydrogel in the solution for 24 h. 2+ 0.03 Solution and TA 0.3 / 0.2 The solvent of the solution was a mixture of glycerol and deionized water.

[0053] Example 3

[0054] A method for preparing a tannic acid-modified protein-based hydrogel comprises the following steps:

[0055] S1. Weigh 1.5 g of SA powder and dissolve it in a mixed solution of 20 mL of deionized water and 20 mL of glycerol, and stir evenly at 70°C to obtain a mixed solution A for use in the next step;

[0056] S2, weigh 10 g of G particles and dissolve them in 40 mL of deionized water, and stir them evenly at 50°C to obtain a mixed solution B for use in the next step;

[0057] S3, weigh 0.8 g of mTG powder and dissolve it in 20 mL of deionized water, and stir it evenly at room temperature to obtain a mixed solution C for use in the next step;

[0058] S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D;

[0059] S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E;

[0060] S6. First, remove the bubbles in the mixed solution E prepared in step S5 by ultrasound; second, pour the mixed solution E into a mold made of plastic and keep it at 45°C for 4 hours to form a G / SA hydrogel; third, place the G / SA hydrogel in Ca 2+ 0.03 The G / SA hydrogel was immersed in TA0.5 / 0.2 The tannic acid-modified protein / sodium alginate hydrogel (G / SA-TA hydrogel) was prepared by immersing the tannic acid-modified protein / sodium alginate hydrogel in the solution for 24 h. 2+ 0.03 Solution and TA 0.5 / 0.2 The solvent of the solution was a mixture of glycerol and deionized water.

[0061] Example 4

[0062] In this Example 4, the G / SA-TA hydrogel prepared in Example 1 was divided into three groups, respectively, 2+ 0.03 , Ca 2 + 0.06 , Ca 2+ 0.09 The G / SA-TA / Ca 2+ Hydrogel.

[0063] The elastic modulus of the hydrogels obtained in Example 1 and this Example 4 is as follows: Figure 3 As shown in the first group of bar graphs in Figure a, the elongation at break is Figure 3 As shown in the first group of bar graphs in Figure b. 0.1 / 0.2 Hydrogel, when Ca 2+ When the concentration increases from 0 to 0.03, the elastic modulus of the hydrogel increases significantly, while the elongation at break does not change significantly. This is because Ca 2+ The SA and TA in the hydrogel system are cross-linked, making the internal structure of the hydrogel more stable, thereby increasing the elastic modulus. 2+ When the concentration continued to increase from 0.03 to 0.09, the elastic modulus and elongation at break of the hydrogel did not change significantly.

[0064] Example 5

[0065] In this Example 5, the G / SA-TA hydrogel prepared in Example 2 was divided into three groups, respectively, 2+ 0.03 , Ca 2 + 0.06 , Ca 2+ 0.09 The G / SA-TA / Ca 2+ Hydrogel.

[0066] The elastic modulus of the hydrogels obtained in Example 2 and this Example 5 is as follows: Figure 3 As shown in the second group of bar graphs in Figure a, the elongation at break is Figure 3 As shown in the second group of bar graphs in Figure b. 0.3 / 0.2 Hydrogel, when Ca2+ When the concentration increases from 0 to 0.09, the elastic modulus of the hydrogel increases and the elongation at break decreases. 0.1 / 0.2 and TA 0.3 / 0.2 The mechanical properties of the two groups of hydrogels show that the increase in TA concentration (0.1 to 0.3) enables the hydrogel to adsorb more Ca 2+ , which also confirms that TA can bind to Ca 2+ Combine.

[0067] Example 6

[0068] A method for preparing a tannic acid-modified protein-based hydrogel comprises the following steps:

[0069] S1. Weigh 1.5 g of SA powder and dissolve it in a mixed solution of 20 mL of deionized water and 20 mL of glycerol, and stir evenly at 70°C to obtain a mixed solution A for use in the next step;

[0070] S2, weigh 10 g of G particles and dissolve them in 40 mL of deionized water, and stir them evenly at 50°C to obtain a mixed solution B for use in the next step;

[0071] S3, weigh 0.8 g of mTG powder and dissolve it in 20 mL of deionized water, and stir it evenly at room temperature to obtain a mixed solution C for use in the next step;

[0072] S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D;

[0073] S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E;

[0074] S6. First, remove the bubbles in the mixed solution E prepared in step S5 by ultrasound; second, pour the mixed solution E into a mold made of plastic and keep it at 45°C for 4 hours to form a G / SA hydrogel; third, place the G / SA hydrogel in Ca 2+ 0.03 After soaking in the solution for 1 min, the gel was rinsed with deionized water. Finally, the G / SA hydrogels were divided into four groups and treated with TA 0 / 0 Solution, TA 0.3 / 0.2 Solution, TA 0.3 / 0.4 Solution, TA 0.3 / 0.6 The solution was soaked for 24 h, and then Ca 2+ 0.06The solution was immersed for 1.5 h to obtain G / SA-TA / Ca 2+ hydrogel; wherein Ca 2+ 0.03 Solution, Ca 2+ 0.06 Solution and TA 0.1 / 0.2 The solvent of the solution was a mixture of glycerol and deionized water.

[0075] The elastic modulus and elongation at break of the hydrogel prepared in Example 6 are as follows: Figure 4 As shown in Figures a and b, as the concentration of glycerol in the TA solution increases, the elastic modulus of the hydrogel decreases continuously, and the elongation at break does not change significantly. This may be because glycerol forms abundant hydrogen bonds with the molecules in the hydrogel, thereby interfering with other interactions between molecules.

[0076] Figure 5 More intuitively, the TA prepared in Example 6 0 / 0 and TA 0.3 / 0.4 The stretching properties of the hydrogel were demonstrated. 0.3 / 0.4 The hydrogel has a wider stretchable range and can withstand twisting, knotting, knot stretching and hanging a weight of 500g, showing excellent tensile properties.

[0077] The hydrogel sample prepared in Example 6 was placed in an environment of 25°C and 10% relative humidity. The mass of the hydrogel was measured at regular intervals and its water retention rate was calculated. The results are as follows: Figure 6 As shown in a. When the glycerol concentration in TA increases from 0.2 to 0.4, the water retention rate of the hydrogel increases significantly. When the glycerol concentration continues to increase to 0.6, the water retention rate of the hydrogel decreases to a certain extent. After 2 days, the hydrogel basically stops losing water. At this time, TA 0.3 / 0.2 and TA 0.3 / 0.4 The water retention rates of the hydrogels were 30.88±1.15% and 56.31±0.80%, respectively. On the sixth day, the hydrogels were bent with tweezers to observe their flexibility. Figure 6 As shown in b, TA 0 / 0 TA 0.3 / 0.4 and TA 0.3 / 0.6 The hydrogels have good flexibility, and TA 0.3 / 0.2 The hydrogel is very brittle and will break when bent. This is because the G / SA hydrogel is 0.3 / 0.2 After solution treatment, its volume shrinks and the water content of the hydrogel decreases. When the glycerol concentration increases, glycerol exerts its water-retaining effect, allowing the hydrogel to maintain flexibility for a longer period of time.

[0078] Figure 7 a is TA 0.3 / 0.2 and TA 0.3 / 0.4Tensile stress-strain curves of the hydrogel in the initial state and after being placed in a -20℃ refrigerator for 1 day. 0.3 / 0.2 After the hydrogel was placed at -20℃ for 1 day, its elastic modulus decreased significantly, and the elongation at break decreased to about 4 / 5 of the original value. 0.3 / 0.4 After the hydrogel was placed at -20℃ for 1 day, its elastic modulus was not significantly different from that in the normal state, and the elongation at break was reduced to about 1 / 2 of the original value. 0.3 / 0.2 and TA 0.3 / 0.4 Hydrogels are soft in their initial state. Figure 7 As shown in b, when one end of the hydrogel is clamped with tweezers, the other end will naturally droop. The two hydrogels were placed at -20℃ for 1 day and then taken out. One end was immediately clamped with tweezers and it was found that TA 0.3 / 0.2 The hydrogel is frozen and very stiff; 0.3 / 0.4 The hydrogel can still sag and maintain good flexibility. When the G / SA hydrogel is immersed in TA solution, part of the water molecules in the hydrogel are replaced by glycerol molecules, realizing the transition from hydrogel to organic hydrogel. Glycerol can form a large number of hydrogen bonds with water molecules, effectively preventing water from freezing below zero degrees, making the hydrogel antifreeze.

[0079] Comparative Example 1

[0080] The difference between this comparative example and Example 1 is that: no "G / SA hydrogel in Ca 2+ 0.03 The remaining steps are the same as in the following step: soak in the solution for 1 min and rinse with deionized water.

[0081] The macroscopic images of the hydrogels prepared in Comparative Example 1 and Example 1 are as follows: Figure 1 As shown, the hydrogel (without Ca 2+ The hydrogel prepared in Example 1 (with Ca 2+ The texture of the pretreatment is uniform and completely transparent. This phenomenon is due to the strong hydrogen bonding when the concentration of the TA solution is high, causing G to precipitate quickly and produce white matter. 2+ After G / SA hydrogel was pretreated with the solution, Ca 2+ It will form a coordination bond with SA in the hydrogel system, forming a protective film on the surface of the hydrogel, slowing down the speed at which TA molecules enter the hydrogel without damaging the hydrogel, and ultimately forming a fully transparent G / SA-TA hydrogel with a uniform texture. 2+ The pretreatment method provides a new idea for improving the tensile strength of G-based hydrogels using high-concentration TA solutions.

[0082] Comparative Example 2

[0083] The difference between this comparative example 2 and example 1 is that: no "G / SA hydrogel in Ca 2+ 0.03 The hydrogel was then immersed in TA 0.1 / 0.2 The solution was immersed for 24 h to obtain G / SA-TA hydrogel. The rest of the steps were the same.

[0084] The tensile modulus and elongation at break of the hydrogels prepared in this comparative example and Examples 1-3 are as follows: Figure 2 As shown in Figures a and b. As the concentration of TA increases, the elastic modulus of the hydrogel increases, and the elongation at break increases first and then decreases. The introduction of TA significantly improves the tensile properties of the hydrogel. This is because the hydrogen bonding between TA and G and SA further cross-links the hydrogel, making the internal structure of the hydrogel more compact. The concentration of TA can be selected according to actual application requirements.

[0085] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing a tannic acid-modified protein-based hydrogel, characterized in that: The following steps are involved: S1, sodium alginate powder is dissolved in a mixed solution of deionized water and glycerol, and stirred evenly at 70°C to obtain a mixed solution A for use in the following step; S2. The protein material is dissolved in deionized water and stirred evenly at 50°C to obtain a mixed solution B for later use; S3, glutaminase was dissolved in deionized water, and stirred evenly at room temperature to obtain a mixed solution C for use in the next step; S4, after the mixed solution A prepared in step S1 is cooled to 50° C., it is mixed with the mixed solution B prepared in step S2, and stirred at 50° C. until the solutions are uniformly mixed, and the volume ratio of the mixed solution A to the mixed solution B is 1:1, to obtain a mixed solution D; S5, mixing the mixed solution D prepared in step S4 and the mixed solution C prepared in step S3, and stirring at 45° C. until the solutions are uniformly mixed, wherein the volume ratio of the mixed solution C to the mixed solution D is 1:4, to obtain a mixed solution E; S6. First, remove bubbles in the mixed solution E prepared in step S5 by ultrasound; Secondly, the mixed solution E was poured into the mold and kept at 45°C for 4 h to form a protein / sodium alginate hydrogel; Again, the protein / sodium alginate hydrogel was immersed in the calcium ion solution for 1 min and then rinsed with deionized water; Finally, the protein / alginate hydrogel was firstly a / b The samples were immersed in the solution for 24 hours, wherein a represents the tannic acid content in the tannic acid solution as a, and the value of a is 0.1, 0.3 or 0.5, and the unit is w / v; b represents the glycerol content in the tannic acid solution as b, and the value of b is 0.2, 0.4 or 0.6, and the unit is v / v; Then soak in calcium ion solution for 1.5h, Ca 2+ The concentration of tannic acid is 0.03 g / mL, 0.06 g / mL or 0.09 g / mL, and the solvents of the calcium ion solution and the tannic acid solution are both a mixture of glycerol and deionized water to prepare tannic acid-modified protein / sodium alginate hydrogel.

2. The method for preparing a tannic acid-modified protein-based hydrogel according to claim 1, characterized in that: In the mixed solution A prepared in step S1, the concentration of sodium alginate is 1.0% wt / v-2.0% wt / v.

3. The method for preparing a tannic acid-modified protein-based hydrogel according to claim 1, characterized in that: In the mixed solution B prepared in step S2, the concentration of the protein material is 10%-15% wt / v.

4. The method for preparing a tannic acid-modified protein-based hydrogel according to claim 1 or 3, characterized in that: The protein material is one or more of gelatin, collagen or casein.

5. The method for preparing a tannic acid-modified protein-based hydrogel according to claim 1, characterized in that: In the mixed solution C prepared in step S2, the concentration of transglutaminase is 0.8%-1.2% wt / v.

6. The method for preparing a tannic acid-modified protein-based hydrogel according to claim 1, characterized in that: The material of the mold in step S6 is plastic.

7. A tannic acid-modified protein-based hydrogel prepared by the method of claim 1.

8. Use of the tannic acid-modified protein-based hydrogel according to claim 7 in the preparation of tissue engineering scaffolds or skin dressings.