A method for repairing a concrete steel plate corner protector
By using epoxy-based chemical grouting materials and ultra-high-performance concrete filling at the bottom of the steel plate, combined with chemical grouting and polyurea layer treatment, the problems of easy corrosion and lax sealing of the steel plate are solved, and stable contact and puddles between the steel plate and the concrete are achieved. Liquid extraction improves construction quality and the service life of steel plates.
Patent Information
- Application Number
- CN202310013600.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-05
AI Technical Summary
Steel plates are prone to rust in flood discharge tunnels, leading to damage. The contact areas between steel plates and concrete are not tightly sealed, which in turn causes damage to the concrete. It is also difficult to drain the liquid in the puddle, affecting the quality of construction.
Add epoxy-based chemical grouting material to the bottom of the steel plate, cut off the damaged parts and install a new steel plate, fill it with epoxy mortar and ultra-high performance concrete, perform chemical grouting and apply a polyurea layer to enhance the sealing between the steel plate and the concrete, and use Artesian aqueducts drain liquids from drainage pits.
It effectively improves the stability and construction quality of the steel plate corner protection, ensures that the repair area can be constructed on dry ground, prevents liquid flow, enhances the sealing between the steel plate and concrete, and extends the service life of the steel plate.
Smart Images

Figure CN115897506B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete steel plate repairing, and in particular to a method for repairing a concrete steel plate corner protector. Background Art
[0002] Steel plates are flat steel plates made by pouring molten steel and pressing them after cooling. However, they still have many shortcomings in actual use. For example, the steel plates in the flood discharge tunnels are severely corroded during long-term use, which can easily cause the steel plates to break. The grouting of the steel plates is not dense, resulting in a poor seal between the upstream contact of the steel plate and the concrete, which is prone to concrete breakage and hollowing out the bottom of the steel plate. Summary of the invention
[0003] The purpose of the present invention is to provide a method for repairing a corner guard of a concrete steel plate, by adding epoxy-based chemical grouting material to the bottom of the steel plate to perform contact grouting on the contact portion between the steel plate and the concrete, thereby further increasing the stability of the corner guard and ensuring the construction quality. The liquid in the puddle is also pumped out to ensure that dry land construction can be carried out in the repair area.
[0004] To achieve the above purpose, the present invention is implemented by the following technical scheme: a method for repairing a concrete steel plate corner protector, comprising the following steps:
[0005] S1: Build a cofferdam on the corner guard to pump out the water in the puddle;
[0006] S2: Cut off the damaged steel plates on the horizontal and vertical surfaces, remove the loose concrete, cut a groove upstream of the damaged part of the horizontal steel plate, and cut a groove downstream of the damaged steel plate on the vertical surface;
[0007] S3: The anchor point position of the new steel plate on the facade is determined and installed at the damaged part of the original facade;
[0008] S4: Fill the epoxy mortar in the groove at the downstream part and perform curing;
[0009] S5: Fill the damaged part of the horizontal surface with ultra-high performance concrete, let the concrete flow from the horizontal surface to the vertical surface, and cure the ultra-high performance concrete;
[0010] S6: Cut a grouting groove at the location where the steel plate is installed on the ultra-high performance concrete surface on the horizontal surface, leave grouting holes at the corresponding position of the steel plate, and install the new steel plate on the horizontal surface;
[0011] S7: Fill the epoxy mortar into the groove upstream of the original damaged part and cure the epoxy mortar;
[0012] S8: Carry out chemical grouting and subsequent maintenance on the new horizontal steel plate, and finally apply a polyurea layer to the new vertical steel plate, the surface of the new horizontal steel plate and the construction operation surface.
[0013] Preferably, in S1, the cofferdam is moved to the corner guard and fixedly installed on one side of the corner guard. The height of the cofferdam is about 0.7m, and a pump is fixedly connected to the cofferdam. The pump is connected to several gravity water pipes, and the water in the puddle is drained through the pump.
[0014] Preferably, the groove cut upstream of the damaged part of the transverse steel plate in S2 is a groove with a width of 5 cm and a depth of 3 cm, and the groove cut downstream of the damaged part of the vertical steel plate is a groove with a width of 3 cm and a depth of 2 cm. The length of the groove upstream of the damaged part of the transverse steel plate and the groove downstream of the damaged part of the vertical steel plate are both consistent with the length of the damaged part.
[0015] Preferably, in S3, the anchor point of the new steel plate of the facade is aligned with the anchor point of the original damaged position of the facade, and the new steel plate of the facade is installed at the original damaged position of the facade, so that the new steel plate and the old steel plate are installed together.
[0016] Preferably, in S4, epoxy mortar is filled into a 3 cm wide, 2 cm deep groove downstream of the damaged portion of the facade steel plate, and the 3 cm wide, 2 cm deep groove is blocked with epoxy mortar, and needs to be kept on the same facade as the intact concrete surface, and wait for the epoxy mortar to cure.
[0017] Preferably, in S5, the damaged part of the horizontal surface is filled with ultra-high performance concrete, and the damaged part of the horizontal surface is blocked by the ultra-high performance concrete. After filling, the ultra-high performance concrete is allowed to flow to the vertical surface by gravity, and then the ultra-high performance concrete on the horizontal surface is smoothed to make the ultra-high performance concrete and the original concrete on the same horizontal line, and wait for the ultra-high performance concrete to solidify.
[0018] Preferably, in S6, a chemical grouting groove is cut out on the ultra-high performance concrete surface of the horizontal surface by a cutting machine. When the chemical grouting groove is from the damaged position of the horizontal surface from left to right, there are multiple forks on the right side. A new horizontal steel plate is installed and installed at the damaged position of the horizontal surface, and the steel plate at the damaged position of the horizontal surface is replaced by the new horizontal steel plate.
[0019] Preferably, in S7, epoxy mortar is filled into a groove 5 cm wide and 3 cm deep upstream of the damaged position on the horizontal surface, the groove 5 cm wide and 3 cm deep is blocked, and it needs to be kept on the same plane as the intact concrete surface, and wait for the epoxy mortar to cure.
[0020] Preferably, the surface of the new transverse steel plate for chemical grouting in S8 has a plurality of grouting holes, and the vertical surface of the grouting holes has grouting pipes, and the spacing distance between each grouting hole is the same.
[0021] The present invention has the following beneficial effects:
[0022] 1. The present invention cuts the damaged steel plate by a cutting machine, and chisels off the old concrete, aligns the anchor point of the new steel plate on the facade with the anchor point of the original damaged position of the facade, installs the new steel plate on the facade at the original damaged position of the facade, ensures the alignment of the position, welds the new steel plate on the facade with the anchor point, installs the new steel plate with the old steel plate, fills the 3cm wide and 2cm deep groove of the downstream part with epoxy mortar, blocks the 3cm wide and 2cm deep groove with epoxy mortar, allows the epoxy mortar to solidify, fills the damaged position of the horizontal surface with ultra-high performance concrete, fills the damaged position of the horizontal surface with ultra-high performance concrete, and after filling, passes through The ultra-high concrete flows to the facade, and then the ultra-high performance concrete on the horizontal surface is smoothed so that the ultra-high performance concrete is at the same level as the original concrete, and wait for the ultra-high concrete to solidify. The new horizontal steel plate is installed and installed at the damaged part of the horizontal surface. The steel plate at the damaged part of the horizontal surface is replaced with the new horizontal steel plate, and the epoxy mortar is filled in the 5cm wide and 3cm deep groove. The 5cm wide and 3cm deep groove is blocked, and the epoxy mortar is waited for to solidify. The new horizontal steel plate is chemically grouted, and finally the surface of the new vertical steel plate and the new horizontal steel plate is coated with a polyurea layer to seal the gap between the steel plate and the concrete to complete the sealing.
[0023] 2. The present invention has multiple gravity water pipes, which are convenient for pumping liquid, draining the liquid in the puddle, and releasing the liquid through a hose connected to the other side of the pump, so as to release the pumped liquid to other places to prevent the liquid from flowing downwards during subsequent work. The height of the cofferdam is about 0.7m, which ensures that dry land construction can be carried out in the repair area. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of the method for repairing the concrete steel plate corner protector. DETAILED DESCRIPTION
[0025] The present invention will be described in detail below in conjunction with the accompanying drawings. Figure 1 As shown, the present invention provides a method for repairing a concrete steel plate corner protector, comprising the following steps:
[0026] S1: A cofferdam is built on the corner guard of the damaged part and fixedly installed on one side of the corner guard. The height of the cofferdam is about 0.7m, and a pump is fixedly connected to the cofferdam. The pump is connected to several gravity water pipes. The water in the puddle is drained by the pump and the liquid is released through the hose connected to the other side of the pump. The pumped liquid is released to other places to prevent the liquid from flowing downward during subsequent work. A cofferdam of about 0.7m is set to ensure that dry land construction can be carried out in the repair area;
[0027] S2: Use a cutting machine to cut off the damaged steel plates, including the damaged steel plates on the horizontal and vertical surfaces, and grind and remove the edges and deformation of the steel plates to make the steel plates easier to weld. Use an electric hammer to chisel out the loose concrete, clean the base surface at the bottom of the corner guard, chisel out the original concrete, and use a cutting machine to cut a groove in the concrete upstream of the damaged part of the horizontal steel plate. The cutting width is about 5 cm, and the electric hammer is used to chisel out, and the chiseling depth is about 3 cm. A 5 cm wide and 3 cm deep groove is cut at the damaged part upstream of the horizontal surface, and the length of the groove is consistent with the length of the damaged part. Similarly, a 3 cm wide and 2 cm deep groove is cut downstream of the damaged part of the vertical steel plate using a cutting machine and an electric hammer, and the length of the groove is consistent with the length of the damaged part.
[0028] S3: The anchor point position of the new steel plate on the facade is determined, and the anchor point of the new steel plate on the facade is aligned with the anchor point of the original damaged part of the facade. The new steel plate on the facade is preferably installed at the damaged part of the original facade by welding with the original anchor bar, so that the new steel plate and the old steel plate are installed together;
[0029] S4: Fill the 3cm wide and 2cm deep groove downstream of the damaged part of the facade with epoxy mortar, plug the 3cm wide and 2cm deep groove with epoxy mortar, and keep it on the same facade as the intact concrete surface, and cure the epoxy mortar until the texture is dry;
[0030] S5: Fill the damaged part of the horizontal surface with ultra-high performance concrete, and fill it evenly. After filling, the ultra-high performance concrete will flow to the vertical surface through the gap between the vertical steel plate and the concrete, and complete the filling of the gap and the damaged part. Then, smooth the ultra-high performance concrete on the horizontal surface, so that the ultra-high performance concrete is on the same horizontal line as the original concrete, and wait for the ultra-high performance concrete to solidify and the ultra-high performance concrete to be cured;
[0031] S6: A chemical grouting groove is cut out on the surface of the ultra-high performance concrete by a cutting machine. The chemical grouting groove is a V-shaped groove. When the chemical grouting groove is from the left to the right of the damaged part on the horizontal surface, there are multiple forks on the right side. The length of the chemical grouting groove runs through the entire damaged part on the horizontal surface. Grouting holes are made for the new steel plate on the horizontal surface. The grouting holes should be located on the grouting groove. The new steel plate on the horizontal surface is installed at the damaged part on the horizontal surface. The installation of the new steel plate on the horizontal surface is preferably installed by welding with the original anchor bar. The steel plate at the damaged part on the horizontal surface is replaced by the new steel plate on the horizontal surface.
[0032] S7: Fill the epoxy mortar in the 5cm wide and 3cm deep groove upstream of the horizontal surface, block the 5cm wide and 3cm deep groove, and keep it on the same plane as the intact concrete surface, and wait for the epoxy mortar to solidify, and finally cure the epoxy mortar;
[0033] S8: Carry out chemical grouting on the new horizontal steel plate. The distances between several grouting holes on the surface of the new horizontal steel plate are the same. Install grouting pipes on the corresponding grouting holes and start grouting. The grouting sequence should be from one end of the V-shaped chemical grouting groove to the other end. Fill in the first grouting pipe, and close it immediately after the second grouting pipe comes out of slurry. Close it immediately after the third grouting pipe comes out of slurry, and so on, until the last grouting pipe comes out of slurry and is closed. After the grouting is completed, subsequent maintenance is carried out. Finally, a polyurea layer is applied to the new vertical steel plate, the new horizontal steel plate and all construction working surfaces. After the maintenance is completed, the construction is terminated.
[0034] Principle of the present invention:
[0035] Use a cutting machine to cut the damaged steel plate and chisel off the old concrete. Align the anchor point of the new steel plate on the facade with the anchor point of the original damaged part of the facade. Install the new steel plate on the facade at the original damaged position of the facade to ensure the alignment of the position. Weld the new steel plate on the facade with the anchor point and install the new steel plate with the old steel plate together. Fill the 3cm wide and 2cm deep groove downstream of the damaged part of the facade with epoxy mortar. Block the 3cm wide and 2cm deep groove with epoxy mortar. Let the epoxy mortar solidify. Fill the damaged part of the horizontal surface with ultra-high performance concrete. After filling, use ultra-high performance concrete to fill the damaged part of the horizontal surface. It flows to the facade, and then the super-high concrete on the horizontal surface is smoothed to make the super-high concrete and the original concrete at the same level, and wait for the super-high concrete to solidify, and install the new horizontal steel plate and install it at the damaged part of the horizontal surface. The steel plate at the damaged part of the horizontal surface is replaced by the new horizontal steel plate, and the epoxy mortar is filled in the 5cm wide and 3cm deep groove upstream of the damaged part of the horizontal surface, and the 5cm wide and 3cm deep groove is blocked, and wait for the epoxy mortar to solidify, and the new horizontal steel plate is chemically grouted. Finally, the new vertical steel plate, the surface of the new horizontal steel plate and all construction work surfaces are coated with a polyurea layer to seal the gap between the steel plate and the concrete to complete the sealing.
[0036] In the initial step of building a cofferdam at the damaged part of the corner guard, there are multiple gravity water pipes to facilitate the pumping of liquid. The liquid in the puddle is drained and the hose connected to the other side of the pump is used to release the pumped liquid to other places to prevent the liquid from flowing downward in subsequent work. The height of the cofferdam is about 0.7m to ensure that dry land construction can be carried out in the repair area.
[0037] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments. It cannot be determined that the specific implementation of the present invention is limited to these descriptions. It should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention.
Claims
1. A method for repairing a concrete steel plate corner protector. It is characterized in that The following steps are involved: S1: Build a cofferdam on the corner guard to pump out the water in the puddle; S2: Cut off the damaged steel plates on the horizontal and vertical surfaces, remove the concrete in the damaged steel plate area, cut a groove upstream of the damaged part of the horizontal steel plate, and cut a groove downstream of the damaged steel plate on the vertical surface; S3: The anchor point position of the new steel plate on the facade is determined and installed at the damaged part of the original facade; S4: Fill the epoxy mortar in the groove at the downstream part and perform curing; S5: Fill the damaged part of the horizontal surface with ultra-high performance concrete, let the concrete flow from the horizontal surface to the vertical surface, and cure the ultra-high performance concrete; S6: A grouting groove is cut at the position where the steel plate is installed on the ultra-high performance concrete surface on the horizontal surface. When the grouting groove is from the damaged position on the horizontal surface to the right, there are multiple forks on the right side. Grouting holes are left at the corresponding positions of the steel plate, and the new steel plate on the horizontal surface is installed; S7: Fill the epoxy mortar into the groove upstream of the original damaged part and cure the epoxy mortar; S8: Carry out chemical grouting and subsequent maintenance on the new horizontal steel plate, and finally apply a polyurea layer to the new vertical steel plate, the surface of the new horizontal steel plate and the construction operation surface.
2. The method for repairing a concrete steel plate corner protector according to claim 1, It is characterized in that In S1, the cofferdam is moved to the corner guard and fixedly installed on one side of the corner guard. The height of the cofferdam is about 0.7m, and a pump is fixedly connected to the cofferdam. The pump is connected to several gravity water pipes, and the water in the puddle is drained through the pump.
3. The method for repairing a concrete steel plate corner protector according to claim 1, It is characterized in that The groove cut upstream of the damaged part of the transverse steel plate in S2 is a groove with a width of 5 cm and a depth of 3 cm, and the groove cut downstream of the damaged part of the vertical steel plate is a groove with a width of 3 cm and a depth of 2 cm. The length of the groove upstream of the damaged part of the transverse steel plate and the groove downstream of the damaged part of the vertical steel plate are both consistent with the length of the damaged part.
4. The method for repairing a concrete steel plate corner protector according to claim 1, It is characterized in that In the above S3, the anchor point of the new steel plate of the facade is aligned with the anchor point of the original damaged position of the facade, and the new steel plate of the facade is installed at the original damaged position of the facade, so that the new steel plate and the old steel plate are installed together.
5. The method for repairing a concrete steel plate corner protector according to claim 3, It is characterized in that In S4, epoxy mortar is filled into the 3 cm wide and 2 cm deep groove downstream of the damaged part of the facade steel plate, and the 3 cm wide and 2 cm deep groove is blocked by epoxy mortar. It needs to be kept on the same facade as the intact concrete surface, and wait for the epoxy mortar to cure.
6. The method for repairing a concrete steel plate corner protector according to claim 1, It is characterized in that In the S5, the damaged part of the horizontal surface is filled with ultra-high performance concrete, and the damaged part of the horizontal surface is blocked by the ultra-high performance concrete. After filling, the ultra-high performance concrete flows to the vertical surface by gravity, and then the ultra-high performance concrete on the horizontal surface is smoothed to make the ultra-high performance concrete and the original concrete on the same horizontal line, and wait for the ultra-high performance concrete to solidify.
7. The method for repairing a concrete steel plate corner protector according to claim 3, It is characterized in that In the S7, epoxy mortar is filled into a groove 5 cm wide and 3 cm deep upstream of the damaged position on the horizontal surface, the groove 5 cm wide and 3 cm deep is blocked, and it needs to be kept on the same plane as the intact concrete surface, and wait for the epoxy mortar to solidify.
8. The method for repairing a concrete steel plate corner protector according to claim 1, It is characterized in that The surface of the new transverse steel plate for chemical grouting in S8 has a plurality of grouting holes, and the vertical surface of the grouting holes has grouting pipes, and the spacing distance between each grouting hole is the same.