A lithium ion battery
By using appropriate conductive agents in lithium-ion batteries to improve the dispersion uniformity of the negative conductive agent and the electron conduction of the positive electrode material, the problem of poor power performance and cycle performance of the lithium-ion battery is solved, and excellent power and cycle performance are achieved. Meet high power and long life requirements.
Patent Information
- Application Number
- CN202211594022.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Existing lithium-ion batteries have insufficient power performance and poor cycle performance, mainly due to the low conductivity of the positive electrode material and uneven dispersion of the negative electrode conductive agent in the aqueous system, resulting in increased internal resistance of the electrode, low utilization of active materials, and increased polarization. Battery cycle life is reduced.
Use conductive agents with high surface oxygen content and relatively low graphitization degree in negative electrode sheets with high conductivity to improve the dispersion uniformity of the negative electrode conductive agent in the aqueous slurry; use in positive electrode sheets with low conductivity The cathode conductive agent with low surface oxygen content and high degree of graphitization increases electron conduction between cathode materials, reduces impedance, and reduces side reactions at high potentials.
It achieves the excellent power performance and cycle performance of lithium-ion batteries and meets the long-life and high-power needs of vehicles. By uniformly dispersing the conductive agent, it improves the electronic conduction network, reduces internal resistance, and reduces side reactions.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a lithium ion battery. Background Art
[0002] Lithium-ion batteries have outstanding advantages such as high energy density, high operating voltage, low self-discharge rate, and environmental friendliness, and can be used as an ideal power source for motors. However, the existing lithium-ion batteries have insufficient power performance and poor cycle performance, which greatly restricts the development of lithium-ion batteries for motors.
[0003] The battery rate performance obtained by the existing technology method is low, and the cycle DCR increases rapidly. The reasons are, on the one hand, that the lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphorus oxide and lithium iron manganese phosphorus oxide, which are the positive electrode materials of lithium-ion batteries, have low conductivity, which increases the internal resistance of the entire electrode, low utilization of active materials, increases polarization when the charge and discharge current increases, and reduces the battery cycle life; on the other hand, the conductive agent is not easy to disperse evenly in the negative electrode water system, resulting in poor electronic conductivity between materials and thus poor kinetic performance. In order to improve the rate performance and cycle life of the battery, the selection of conductive agents for existing batteries is optimized. Summary of the invention
[0004] One of the purposes of the present invention is to provide a lithium ion battery in view of the shortcomings of the prior art, wherein a conductive agent having a high surface oxygen content and a relatively low degree of graphitization is used in a negative electrode sheet with higher conductivity to improve the dispersion uniformity of the negative electrode conductive agent in an aqueous slurry, and a positive electrode conductive agent having a low surface oxygen content and a high degree of graphitization is used in a positive electrode sheet with lower conductivity to increase the electronic conduction between the positive electrode materials and reduce the impedance. In addition, the conductive agent contains fewer oxygen functional groups, which reduces the side reaction between the oxygen-containing functional groups and the electrolyte at high potential, thereby obtaining a battery with excellent power performance and cycle performance.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A lithium-ion battery comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode coating arranged on the surface of the positive electrode current collector, wherein the positive electrode coating comprises a positive electrode conductive agent, and the surface oxygen content of the positive electrode conductive agent is 0.01% to 3%. The negative electrode sheet comprises a negative electrode current collector and a negative electrode coating arranged on the surface of the negative electrode current collector, wherein the negative electrode coating comprises a negative electrode conductive agent, and the surface oxygen content of the negative electrode conductive agent is 3% to 10%.
[0007] Preferably, the specific surface area of the positive electrode conductive agent is 55-90m 2 / g, the interlayer spacing is 0.336~0.36nm, and the crystal size is 2.0~3.5nm.
[0008] Preferably, the weight fraction of the positive electrode conductor in the positive electrode coating is 0.01% to 6%.
[0009] Preferably, the specific surface area of the negative electrode conductive agent is 55-90m 2 / g, the interlayer spacing is 0.36-0.38nm, and the crystal size is 1.0-2.0nm.
[0010] Preferably, the weight fraction of the negative electrode conductive agent in the negative electrode coating is 0.5% to 3.0%.
[0011] Preferably, the positive electrode coating also includes a positive electrode active material, and the positive electrode active material includes one or more of a nickel cobalt lithium manganese oxide ternary material, a nickel cobalt lithium manganese oxide ternary material modified by doping and coating, a lithium iron phosphate material, a lithium iron manganese phosphate material, a carbon-coated lithium iron phosphate material, an iron manganese phosphate material, a lithium manganese oxide material, and a lithium cobalt oxide material.
[0012] Preferably, the chemical formula of the nickel-cobalt-lithium-manganese oxide ternary material is Li x Ni a Co b Mn c O2, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,0≤c≤1,a+b+c=1。
[0013] Preferably, the chemical formula of the lithium manganese iron phosphate material is Li x Mn a Fe b PO4, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,a+b=1。
[0014] Preferably, the negative electrode coating further includes a negative electrode active material, and the negative electrode active material includes one or more of artificial graphite, natural graphite, silicon, silicon oxide, and tin.
[0015] Preferably, the positive electrode conductive agent is at least one of activated carbon, carbon black, carbon nanotubes, graphite, soft carbon, hard carbon, and amorphous carbon and / or the negative electrode conductive agent is at least one of activated carbon, carbon black, carbon nanotubes, graphite, soft carbon, hard carbon, and amorphous carbon.
[0016] Preferably, the negative electrode coating further includes a negative electrode active material, and the negative electrode active material includes one or more of artificial graphite, natural graphite, silicon, silicon oxide, and tin.
[0017] Preferably, the positive electrode coating further includes a binder, and the negative electrode coating further includes a binder, and the binder includes one of styrene-butadiene rubber, polyacrylamide, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylonitrile, and polyimide.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: the lithium ion battery of the present invention uses a conductive agent with a high surface oxygen content and a relatively low degree of graphitization in the negative electrode sheet with a higher conductivity, thereby improving the uniformity of dispersion of the negative electrode conductive agent in the aqueous slurry. The negative electrode conductive agent with more oxygen functional groups has good hydrophilicity and is easy to form hydrogen bonds with solvent molecules to combine, thereby making the negative electrode conductive agent uniformly dispersed in the slurry, making the electronic conductive network of the electrode sheet more perfect, and reducing the internal resistance. The positive electrode conductive agent with a low surface oxygen content and a high degree of graphitization is used in the positive electrode sheet with a lower conductivity, thereby increasing the electronic conduction between the positive electrode materials and reducing the impedance. Moreover, the conductive agent contains fewer oxygen functional groups, which reduces the side reaction between the oxygen-containing functional groups and the electrolyte at high potential, thereby obtaining a battery with excellent power performance and cycle performance. DETAILED DESCRIPTION
[0019] The present invention will be described in further detail below in conjunction with specific implementation modes, but the implementation modes of the present invention are not limited thereto.
[0020] A lithium-ion battery comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode coating disposed on the surface of the positive electrode current collector, wherein the positive electrode coating comprises a positive electrode conductive agent, wherein the surface oxygen content of the positive electrode conductive agent is 0.01% to 3%, the interlayer spacing of the positive electrode conductive agent is 0.336 to 0.36 nm, and the crystal size of the positive electrode conductive agent is 2.0 to 3.5 nm. The negative electrode sheet comprises a negative electrode current collector and a negative electrode coating disposed on the surface of the negative electrode current collector, wherein the negative electrode coating comprises a negative electrode conductive agent, wherein the surface oxygen content of the negative electrode conductive agent is 3% to 10%, the interlayer spacing of the negative electrode conductive agent is 0.36 to 0.38 nm, and the crystal size of the negative electrode conductive agent is 1.0 to 2.0 nm.
[0021] Since the conductivity of lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium manganese oxide, lithium iron phosphorus oxide and lithium iron manganese phosphorus oxide, which are used as positive electrode materials of ion batteries, is low, the internal resistance of the entire electrode increases, the utilization rate of active materials is low, and when the charge and discharge current increases, the polarization increases and the battery cycle life decreases. In order to ensure that the battery electrode has good charge and discharge performance, a certain amount of conductive agents such as furnace black, acetylene black or carbon nanotubes are usually added when making the positive electrode sheet to increase the conductivity between the active material and the current collector and between the active material particles, thereby improving the charge and discharge efficiency of the battery. For negative electrode materials such as graphite and natural graphite, although they have certain conductivity, when the battery is charged and discharged at a high rate, the gaps between the graphite particles reduce the rate performance of the battery. Therefore, conductive carbon black, acetylene black and other conductive agents with smaller particles (before adding the electrode slurry, the particle diameter is usually 40-400 nanometers) are added to the electrode slurry when making the electrode. It is hoped that these conductive carbon black, acetylene black and other conductive agents with smaller particles can collect microcurrents between graphite particles and between graphite and the current collector, reduce the contact resistance of the electrode, and accelerate the migration rate of electrons, so as to effectively increase the migration rate of lithium ions in the electrode material and increase the conductivity of the electrode.
[0022] When making pole pieces, the active material, conductive agent, binder and solvent are mixed in proportion, and the evenly mixed electrode slurry is loaded on the positive and negative current collectors. After drying, rolling and cutting, the positive and negative pole pieces are obtained. The pole pieces and the isolation film are then wound to form a core. The core is wrapped with aluminum-plastic film to form a semi-finished battery cell, and then the electrolyte is injected. After the formation and capacity separation steps, the finished lithium-ion battery is obtained, and the electrical performance is tested.
[0023] In actual production, it is found that the particle diameter of the conductive carbon black used in the negative electrode is small, usually only 40-400 nanometers, with a large specific surface area and high surface energy. The particles are easy to agglomerate to form agglomerates with a diameter of up to 10 microns, and the agglomerates formed cannot be effectively dispersed. In the electrode slurry, the conductive agent forms large particles with a diameter of more than 18 microns, resulting in obvious uneven dispersion of the conductive agent in the electrode slurry. On the one hand, it affects the stability and rheological properties of the electrode slurry, and on the other hand, it also makes the conductive carbon black on the pole piece unevenly distributed. The conductivity of the battery pole piece made from this is uneven, and the resistivity changes greatly, so that the battery polarization phenomenon is easy to occur when the prepared battery is discharged at a high rate, the discharge capacity is low, and the rate discharge performance is poor. In actual applications, it is found that the positive electrode is prone to oxidation side reactions under high temperature and high voltage, which increases the impedance and deteriorates the long-term performance.
[0024] Therefore, the purpose of the present invention is to overcome the shortcomings of poor rate performance and poor cyclicity in the prior art. The lithium ion battery of the present invention uses a conductive agent with a high surface oxygen content and a relatively low graphitization degree in the negative electrode sheet with higher conductivity. The conductive agent with more surface oxygen functional groups has good hydrophilicity and is easy to form hydrogen bonds with solvent molecules to be combined, so that the conductive agent is more evenly dispersed in the slurry, so that the electrochemical performance of the obtained negative electrode sheet is better, the dispersion uniformity of the negative electrode conductive agent in the aqueous slurry is improved, the electronic conduction network is improved, and the electronic resistance is reduced. Since the negative electrode material itself has a high degree of graphitization, the conductive agent uses a material with a relatively low degree of graphitization to reduce costs. In the positive electrode sheet with lower conductivity, a positive electrode conductive agent with a low surface oxygen content and a high degree of graphitization is used to increase the electronic conduction between the positive electrode materials, reduce the impedance, and the conductive agent contains fewer oxygen functional groups, which reduces the side reaction between the oxygen-containing functional groups and the electrolyte at high potential, thereby obtaining a battery with excellent power performance and cycle performance. It can meet the needs of long life and high power of vehicles.
[0025] In a lithium-ion battery of this embodiment, the negative electrode sheet uses a negative electrode conductive agent with many oxygen functional groups. The negative electrode conductive agent with many oxygen functional groups has good hydrophilicity and is easy to form hydrogen bonds with solvent molecules to combine, so that the negative electrode conductive agent is evenly dispersed in the slurry to obtain a negative electrode sheet with good electrochemical performance; the positive electrode sheet uses a positive electrode conductive agent with few oxygen functional groups to reduce the probability of side reactions between the positive electrode conductive agent and the electrolyte, avoid impedance increase, and make the battery have excellent power performance and cycle performance. Preferably, the surface oxygen content of the positive electrode conductive agent is 0.01% to 1%, 1% to 2%, 2% to 3%, specifically, the surface oxygen content of the positive electrode conductive agent is 0.01%, 0.05%, 0.09%, 0.1%, 0.5%, 0.9%, 1.5%, 2.5%, 2.8%. Preferably, the surface oxygen content of the negative electrode conductive agent is 3% to 5%, 5% to 7%, 7% to 10%. Specifically, the surface oxygen content of the negative electrode conductive agent is 3%, 3.5%, 3.8%, 4%, 4.5%, 4.9%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%.
[0026] The specific surface area of the positive electrode conductive agent in this embodiment is 55-90m 2 / g, the interlayer spacing is 0.336-0.36nm, and the crystal size is 2.0-3.5nm. Preferably, the specific surface area of the positive electrode conductive agent is 55m 2 / g, 58m 2 / g, 60m 2 / g, 62m 2 / g, 65m 2 / g, 68m 2 / g, 70m 2 / g, 72m 2 / g, 75m 2 / g, 80m 2 / g, 85m 2 / g, 90m 2 / g. Specifically, the interlayer distances are 0.336nm, 0.34nm, 0.35nm, 0.36nm. Specifically, the crystal sizes are 2.0nm, 2.4nm, 2.8nm, 3.0nm, 3.2nm, 3.4nm, 3.5nm.
[0027] Preferably, the weight fraction of the positive electrode conductive agent in the positive electrode coating is 0.01% to 6%. The weight fraction of the positive electrode conductive agent in the positive electrode coating is 0.01%, 0.1%, 0.5%, 0.9%, 1%, 2%, 3%, 4%, 5%, 6%.
[0028] Preferably, the specific surface area of the negative electrode conductive agent is 55-90m 2 / g, the interlayer spacing is 0.36-0.38nm, and the crystal size is 1.0-2.0nm. Preferably, the specific surface area of the negative electrode conductive agent is 55m 2 / g, 58m 2 / g, 60m 2 / g, 62m 2 / g, 65m 2 / g, 68m 2 / g, 70m 2 / g, 72m 2 / g, 75m 2 / g, 80m 2 / g, 85m 2 / g, 90m 2 / g. The interlayer spacing is 0.36nm, 0.37nm, 0.38nm. The crystal size is 1.0nm, 1.2nm, 1.4nm, 1.5nm, 1.7nm, 1.9nm, 2.0nm.
[0029] Preferably, the weight fraction of the negative electrode conductive agent in the negative electrode coating is 0.5% to 3.0%. Preferably, the weight fraction of the negative electrode conductive agent in the negative electrode coating is 0.5% to 1.5%, 1.5% to 2%, 2% to 3%. Specifically, the weight fraction of the negative electrode conductive agent in the negative electrode coating is 0.5%, 0.8%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 2.8%, 3.0%.
[0030] Preferably, the positive electrode coating also includes a positive electrode active material, and the positive electrode active material includes one or more of a nickel cobalt lithium manganese oxide ternary material, a nickel cobalt lithium manganese oxide ternary material modified by doping and coating, a lithium iron phosphate material, a lithium iron manganese phosphate material, a carbon-coated lithium iron phosphate material, an iron manganese phosphate material, a lithium manganese oxide material, and a lithium cobalt oxide material.
[0031] Preferably, the chemical formula of the nickel-cobalt-lithium-manganese oxide ternary material is Li x Ni a Co b Mn c O2, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,0≤c≤1,a+b+c=1。
[0032] Preferably, the chemical formula of the lithium manganese iron phosphate material is Li x Mn a Fe b PO4, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,a+b=1。
[0033] Preferably, the negative electrode coating further includes a negative electrode active material, and the negative electrode active material includes one or more of artificial graphite, natural graphite, silicon, silicon oxide, and tin.
[0034] Preferably, the positive electrode conductive agent is at least one of activated carbon, carbon black, carbon nanotubes, graphite, soft carbon, hard carbon, and amorphous carbon and / or the negative electrode conductive agent is at least one of activated carbon, carbon black, carbon nanotubes, graphite, soft carbon, hard carbon, and amorphous carbon.
[0035] Conductive carbon black material performance test
[0036] 1. Specific surface area (BET) test
[0037] The characterization of the micro-mesoporous structure in this patent is completed by nitrogen adsorption test, taking the specific surface area as an indicator, and the corresponding test standard is GB / T19587-2017. The dispersion of the conductive agent in the slurry is affected not only by the surface functional groups but also by the structural degree and specific surface area. If the structural degree and surface properties are the same, the one with a large specific surface area is difficult to disperse in the slurry;
[0038] 2. X-ray diffraction (XRD)
[0039] Data were collected using a PANaIytica IX' PertPRO diffractometer coupled to a PANaIytica IX' Celerator detector. The diffractometer had the characteristics shown in Table 1 below:
[0040] Table 1: Instrument data and measurement parameters
[0041] Table 1
[0042] instrument PANalytical X'Pert PRO X-ray detector PANalytical X'Celerator X-ray Source Cu-Kα Generator parameters 45kV-40mA Scan speed 0.07 degrees / s (for Lc and c / 2) Diverging slits 1 degree Sample rotation 60rpm
[0043] Data were analyzed using PaNaiyticai X'Pert X'Pert High Score Plus software.
[0044] Layer spacing c / 2
[0045] The interlayer spacing c / 2 is determined by X-ray diffraction. The angular position of the maximum peak of the (002) reflection curve is determined, and by applying the Bragg equation, the interlayer spacing is calculated (Klug and Alexander, X-ray diffraction Procedures, John Wiley & Sons Inc., New York, London (1967)). In order to avoid the problems caused by the low absorption coefficient of carbon, instrument calibration and the non-planarity of the sample, internal standard silicon powder is added to the sample, and the graphite peak position is recalculated based on the position of the silicon peak. The graphite sample is mixed with the silicon standard powder by adding a mixture of polyethylene glycol and ethanol. The slurry obtained is then coated on a glass plate and dried by a blade with a spacing of 150 μm.
[0046] Crystal size Lc
[0047] The crystal size is determined by analyzing the [002J diffraction curve and measuring the width of the peak curve at half peak. As proposed by Scherrer, peak broadening should be affected by crystal size. However, broadening is also affected by other factors such as X-ray absorption, Lorentz polarization and atomic scattering factors. Several methods have been proposed to take these effects into account by using an internal silicon standard and applying a correction function to the Scherrer formula. For the present invention, the method proposed by Iwashita is used (N. Iwashita, C. Rae Park, H. Fujimoto, M. Shiraishi and M. Inagaki, Carbon 42, 701-714 (2004)). Sample preparation is the same as the above-mentioned c / 2 determination.
[0048] 3. Oxygen content is tested by X-ray photoelectron spectroscopy (XPS)
[0049] The elemental composition and species formation of the surface of the measured carbonaceous material were determined using an X-ray photoelectron spectrometer (SIGMAProbe II XPS) equipped with an ALPHA 110 hemispherical electron energy analyzer (average radius of 110 mm). The sample was placed and pressed into a bowl-shaped aluminum sample holder (6 mm in diameter) by aluminum paper without any stickers. A MgKα X-ray source (1253.6 eV) operating at 200 W was used to irradiate the sample under vacuum (<10-7 Pa). The intensity and kinetic energy of the emitted photoelectrons displayed by the electron analyzer provide information about the chemical properties of the atoms present on the surface. The sample emission angle and the light source to the analyzer angle were 0 degrees and 50 degrees, respectively, the lens mode was large area XPS, and the dwell time and energy step were 50 ms and 0.1 eV, respectively. The analyzer was operated in a fixed analyzer transmission mode, where the pass energy was set to 50 eV for collecting the measurement spectrum (average of 9 scans) and was set to 20 eV for collecting high-resolution spectra (average of 27 scans).
[0050] The collected XPS spectrum was referenced to the aliphatic carbon C1s signal at 285.0 eV and fitted by CASAXPS software with a Gaussian Lorentzian line shape after Shirley background subtraction. All fitting parameters except the peak intensity were constrained, and the binding energy of the signal components was assigned according to literature 1. The C1s signal and the O1s signal were quantitatively analyzed by considering the peak area in the high-resolution spectrum, and corrected for the photoionization cross section, asymmetry function, attenuation length and analyzer transmission function of Scofield 2,3,4,5. The relative sensitivity factors calculated for the C1s signal and the O1s signal were 1.00, 3.30 and 0.52, respectively. The maximum uncertainty of the measured binding energy is equal to 0.2 eV6.
[0051] The above preparation results are recorded in Table 2.
[0052] Table 2
[0053]
[0054] Example 1
[0055] Battery preparation:
[0056] The positive electrode material powder, conductive carbon, carbon nanotubes and PVDF were mixed in a specified ratio, and then NMP was added in a high-speed mixer and uniformly mixed into a slurry with a solid content of 74%. The slurry was coated on one side of an aluminum foil with a thickness of 13 microns using a transfer coater and dried to maintain a coating weight per unit area of 20.0 mg / cm after drying. 2 Then, the same process is adopted on the other side of the aluminum foil to coat and dry to obtain a semi-finished positive electrode sheet.
[0057] Artificial graphite powder, conductive carbon, carbon nanotubes, CMC and SBR were mixed in a specified ratio, and then deionized water was added in a high-speed mixer and uniformly mixed into a slurry with a solid content of 48%. The slurry was coated on one side of a copper foil with a thickness of 8 microns using a transfer coater and dried to maintain a unit area coating weight of 18.1 mg / cm after drying. 2 Then, the same process is adopted on the other side of the copper foil to coat and dry to obtain a negative electrode semi-finished product.
[0058] The exposed metal foil of the pole piece is processed and welded into a pole ear, and then wound with a separator to form a winding core. The winding core is wrapped with an aluminum-plastic film to form a semi-finished battery cell, and then an electrolyte is injected, and a finished lithium-ion battery is obtained through formation and capacity separation steps.
[0059] With reference to Example 1, Examples 2-10 and Comparative Example 1 were prepared, and the prepared secondary batteries were subjected to performance tests. The test results are recorded in Table 3.
[0060] Pole performance test
[0061] 1. Positive electrode sheet resistivity test
[0062] The ACCFilm film resistor meter is used to directly measure the overall resistivity of the electrode. The resistance measured at this time includes the resistance of the probe itself, the contact resistance between the probe and the coating, the coating resistance, the contact resistance between the coating and the current collector, and the resistance of the current collector itself. During the measurement process, the main parameters include the loading current and the pressure applied by the probe. The corresponding test standard is GB / T19587-2017. The test principle is Ohm's theorem: R=U / I. If the conductive agent is unevenly dispersed in the dispersant and forms larger agglomerates, the conductive agent on the electrode electrode sheet thus made will also be unevenly dispersed, resulting in less or no conductive agent in the local area, thereby increasing the resistivity of the electrode sheet. Therefore, the smaller the resistivity, the more evenly the conductive agent is dispersed on the electrode sheet.
[0063] Battery performance test
[0064] 1. Power performance: 25 degrees 50% SOC 2C rate discharge for 30 seconds to measure DCR (2C-30s50% SOC DCR@25℃):
[0065] First, the 1C capacity is tested. The lithium-ion battery is placed in a constant temperature environment of 25°C for 1h, and 1C / 1C charge and discharge are performed using the nominal capacity. After constant current charging to a voltage of 4.3V at a charging current of 1C, the charging cut-off current is 0.05C at a constant voltage of 4.3V. After standing for 15min, constant current discharge is performed to 2.8V at a discharge current of 1C. The discharge capacity is the 1C capacity C0; then the SOC is adjusted to 50%, and 1C0 is charged at a constant current to a voltage of 4.3V, and the charging cut-off current is 0.05C0 at a constant voltage of 4.3V. After standing for 15min, 1C0 is discharged at a constant current for 30min; 25℃ 50% SOCDCR test: The lithium-ion battery is placed in a constant temperature environment of 25℃ for 1h, and 2C is discharged for 30s. The voltage in the last second before discharge is recorded as V1, and the voltage for 30s of discharge is recorded as V2. The discharge DCR of 25℃ 50% SOC is (V1-V2) / (2C0).
[0066] 2. 25 degrees 50% SOC 15C rate discharge for 8 seconds to measure DCR (15C-8s50% SOC DCR@25℃):
[0067] First, the 1C capacity is tested. The lithium-ion battery is placed in a constant temperature environment of 25°C for 1h, and 1C / 1C charge and discharge are performed using the nominal capacity. After constant current charging to a voltage of 4.3V at a charging current of 1C, the charging cut-off current is 0.05C at a constant voltage of 4.3V. After standing for 15min, constant current discharge is performed to 2.8V at a discharge current of 1C. The discharge capacity is the 1C capacity C0; then the SOC is adjusted to 50%, and 1C0 is charged at a constant current to a voltage of 4.3V, and the charging cut-off current is 0.05C0 at a constant voltage of 4.3V. After standing for 15min, 1C0 is discharged at a constant current for 30min; 25°C 10% SOCDCR test: The lithium-ion battery is placed in a constant temperature environment of 25°C for 1h, and discharged at 15C for 8s. The voltage in the last second before discharge is recorded as V1, and the voltage for 8s of discharge is recorded as V2. The discharge DCR of 50% SOC at 25°C is (V1-V2) / (15C0).
[0068] 3. Cycle performance: 45 degree cycle performance test:
[0069] First, in an environment of 45°C, the first charge and discharge were carried out. After constant current charging at a charging current of 1C to a voltage of 4.3V, the charging cutoff current was 0.05C at a constant voltage of 4.3V. After standing for 15 minutes, constant current discharge was carried out at a discharge current of 1C to 2.8V. The discharge capacity of the first cycle was recorded as C1; then charge and discharge cycles were carried out until the capacity decayed to 80% C1, and the number of cycles corresponding to the discharge capacity retention rate of 80% was recorded.
[0070] 4. Cyclic DCR and DCR growth test:
[0071] After the first cycle of 45 degree cycle in 3 is charged to 4.3V with 1C1 constant current, the charging cut-off current is 0.05C0 at 4.3V constant voltage. After standing for 15 minutes, the voltage V3 is one second before the discharge starts. The voltage V4 is recorded after 30s of 1C0 constant current discharge. The first cycle (capacity maintained 100%) discharge DCR1 is (V3-V4) / C1. The same test obtains DCR2 after the cycle capacity decays by 80%, and the cycle DCR growth is (DCR2-DCR1) / DCR1×100%.
[0072] Table 3
[0073]
[0074] It can be concluded from Table 2 that the surface oxygen content of conductive carbons 1-3 is between 0.77 and 1.51, which has a lower surface oxygen content. The surface oxygen content of conductive carbons 4 to 6 is between 6.28 and 7.02, which has a lower surface oxygen content. Embodiments 1-10 of the present invention are mixed and matched according to the above-mentioned conductive carbons 1-6 to prepare secondary batteries, and the performance of the secondary batteries is tested. The results are shown in Table 3. From Table 3, it can be concluded that when the positive electrode sheet uses one of the conductive carbons 1 to 3 and the negative electrode sheet uses one of the conductive carbons 4 to 6, the prepared secondary battery has better performance. At a temperature of 45°C, 1C / 1C cycle charge and discharge are performed. When the capacity retention rate is reduced to 80%, the number of cycles achieved is more than 1700, the DCR is only 57.7mohm, and the DCR growth rate is only less than 160%. When both the positive and negative electrodes in the battery use conductive carbons 1 to 3 or conductive carbons 4 to 6, such as in Examples 1, 2, 4, 6, 7, and 9, one of the electrodes of the prepared secondary battery has a higher resistance, resulting in a faster increase in DCR and poor performance after multiple charge and discharge cycles.
[0075] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A lithium ion battery, characterized in that , including a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode coating arranged on the surface of the positive electrode current collector, the positive electrode coating includes a positive electrode conductive agent, and the surface oxygen content of the positive electrode conductive agent is 1% to 2%, the negative electrode sheet includes a negative electrode current collector and a negative electrode coating arranged on the surface of the negative electrode current collector, the positive electrode coating also includes a positive electrode active material, the positive electrode active material includes a nickel cobalt lithium manganese oxide ternary material, a nickel cobalt lithium manganese oxide ternary material modified by doping and coating, a lithium iron phosphate material, and a lithium iron manganese phosphate The negative electrode coating comprises a negative electrode conductive agent, and the surface oxygen content of the negative electrode conductive agent is 5% to 7%. The negative electrode coating also comprises a negative electrode active material, and the negative electrode active material comprises one or more of artificial graphite, natural graphite, silicon, silicon oxide, and tin. The positive electrode conductive agent and the negative electrode conductive agent both comprise carbon black, and the specific surface area of the positive electrode conductive agent is 55-90 m 2 / g, the interlayer spacing is 0.336-0.36nm, the crystal size is 2.0-3.5nm, the weight fraction of the positive electrode conductive agent in the positive electrode coating is 0.01%-6%, and the specific surface area of the negative electrode conductive agent is 55-90m 2 / g, the interlayer distance is 0.36-0.38nm, the crystal size is 1.0-2.0nm, and the weight fraction of the negative electrode conductive agent in the negative electrode coating is 0.5%-3.0%.
2. The lithium-ion battery according to claim 1, characterized in that The chemical formula of the nickel-cobalt-lithium-manganese oxide ternary material is Li x Ni a Co b Mn c 02, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,0≤c≤1,a+b+c=1。 3. The lithium-ion battery according to claim 1, characterized in that The chemical formula of the lithium manganese iron phosphate material is Li x Mn a Fe b Po4, of which 0.85 <x<1.2,0≤a≤1,0≤b≤1,a+b+c=1。