A heterobinuclear copper-based catalyst for synthesizing vinyl chloride, and its preparation method and application
Through the preparation method of heterobinuclear copper-based catalyst, the toxicity and inactivation of catalysts in vinyl chloride synthesis are solved, and the catalytic effect with high activity and long life is achieved, which is suitable for the industrial production of vinyl chloride.
Patent Information
- Application Number
- CN202211633978.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The existing vinyl chloride synthesis catalysts have high toxic and volatile mercury chloride catalysts that pose a threat to the environment and health. The cost of precious metal catalysts is high, and non-precious metal catalysts such as copper catalysts are fast deactivating, resulting in insufficient stability and activity.
Using the preparation method of heterobinuclear copper-based catalyst, the heterobinuclear complex is formed by bridging reaction between the copper mononuclear complex and the second metal mononuclear complex, and combined with the porous carbon support, and the carrier stability and metal are improved by microwave treatment. The dispersibility of the active components forms a catalyst with high activity and stability.
The ultra-long stability and ultra-high activity of the catalyst are achieved, which significantly improves the efficiency of vinyl chloride synthesis reaction and the economic applicability of the catalyst, and avoids the inactivation problem of traditional catalysts.
Smart Images

Figure FDA0005045362110000021 
Figure FDA0005045362110000031 
Figure FDA0005045362110000032
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst technology preparation, and specifically relates to a copper-based catalyst and a preparation method thereof and application thereof in vinyl chloride synthesis reaction. Background Art
[0002] The production of vinyl chloride monomer (VCM) is a very important industrial process. Polyvinyl chloride (PVC) polymerized from VCM is a raw material chemical for various plastics. Due to the energy characteristics of rich coal, poor oil and little gas, nearly 80% of China's PVC production comes from the calcium carbide acetylene process. At present, the industrial catalyst for synthesizing vinyl chloride is a highly toxic and volatile mercuric chloride catalyst, which seriously harms the ecological environment and people's life and health. Therefore, the development of environmentally friendly non-mercury catalysts is urgent and indispensable.
[0003] Precious metal Au, Ru, and Pd catalysts have high catalytic activity, but their further development is limited by cost issues. The development of non-precious metal catalysts with cost advantages is also potential. Cu catalysts, as representatives of non-precious metal catalysts, have good initial activity, but the rapid deactivation of copper catalysts is also an inevitable problem. The regulation of the electronic structure of metal active components can change the ability of reactants and products to adsorb, activate, and desorb, thereby significantly improving the activity and stability of the catalyst. Therefore, the regulation of the electronic structure of the active components of the catalyst is of great significance.
[0004] Carrier optimization, additive addition, ligand coordination, etc. are commonly used modification methods for copper-based catalysts for vinyl chloride synthesis. Chinese patent (CN 111715253 A) discloses a method for modifying activated carbon carriers by doping with boron and nitrogen heteroatoms. The modified carrier can not only enhance the interaction with the copper complex and prevent the loss of the copper complex, but also regulate the adsorption performance of acetylene and hydrogen chloride gas. Under the synergistic effect of the two, the activity and stability of the catalyst are improved. Chinese patent (CN 110961112A) discloses a method for preparing a copper-based catalyst with a second metal additive added. Bismuth, barium, manganese, iron, magnesium, etc. are added as the second metal additive to the copper-based catalyst loaded on alumina and applied to the reaction of synthesizing vinyl chloride, achieving good results. A Chinese patent (CN 111151299 A) discloses an alcohol copper complex catalyst, a preparation method thereof, and an application thereof in vinyl chloride synthesis reaction. Copper salt and polyol compounds are mixed and loaded on a porous solid carrier, and the oxygen atoms of the alcohol compound are used to form a coordination structure with the copper atoms, thereby improving the activity and stability of the copper-based catalyst.
[0005] Compared with modifying copper catalysts by modifying carriers or adding metal additives, ligand coordination has obvious advantages in improving activity and stability. The addition of ligands can form stable complexes, which can not only regulate the electronic structure of metals, thereby inhibiting the reduction of active components, but also improve the dispersion of active components on the carrier surface and inhibit carbon deposition. Today, the research focus of coordination chemistry has gradually evolved from complexes containing only a single central atom to polynuclear complexes containing multiple central atoms. In polynuclear complexes, two or more metal atoms are connected by bridging ligands. These metal atoms can be the same, that is, homopolynuclear complexes; or they can be different, that is, heteropolynuclear complexes. Compared with mononuclear complexes, polynuclear complexes can exhibit unique physical properties, chemical properties and physiological activities, thus having better performance. In the field of catalysis, compared with homopolynuclear complexes, heterobinuclear complexes not only have the function of stabilizing active components with ligands to improve activity, but also can utilize the synergistic effect between different metals to regulate electronic structures that are more conducive to catalytic reactions, thereby further improving the activity and stability of the catalyst. Summary of the invention
[0006] The object of the present invention is to provide a heterobinuclear copper-based catalyst with ultrahigh stability and catalytic activity, a preparation method thereof and an application thereof in a vinyl chloride synthesis reaction.
[0007] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:
[0008] In a first aspect, the present invention provides a method for preparing a heterobinuclear copper-based catalyst for synthesizing vinyl chloride, comprising the following steps:
[0009] Step 1: Synthesis of copper mononuclear complex: copper salt, bridging ligand and solvent A are mixed and placed in a magnetic stirrer for stirring at a speed of 100 to 2000 rpm for 2 to 24 hours to form a suspension A; the molar ratio of the copper element contained in the copper salt to the bridging ligand is 1:0.9 to 2; the feed ratio of the bridging ligand to the solvent A is 5 to 20 g:100 mL; the copper salt is selected from at least one of a monovalent copper salt and a divalent copper salt;
[0010] Step 2: Synthesis of the second metal mononuclear complex: The second metal salt, the ionic liquid as the terminal ligand and the solvent B are mixed and placed in a magnetic stirrer for stirring reaction, the stirrer speed is 200-2000rpm, the stirring time is 2-24h, and then the mixture is allowed to stand for stratification, the lower layer of liquid is separated by a separatory funnel, and then it is repeatedly washed with deionized water for more than three times to obtain a mixed solution B; wherein the molar ratio of the ionic liquid to the second metal ion contained in the second metal salt is 1:0.9-2; the feed ratio of the ionic liquid to the solvent B is 7-20g:100ml; the second metal is selected from one of potassium, magnesium, aluminum, chromium, manganese, iron, cobalt, nickel, zinc, gallium, zirconium, ruthenium, palladium, silver, cadmium, indium, tin, cesium, barium, and platinum;
[0011] Step 3: Synthesis of heterobinuclear complex: Place the suspension A obtained in step 1 into a vortex mixing oscillator, slowly add the mixed solution B obtained in step 2 thereto, and continue stirring for 2 to 24 hours. The speed of the vortex mixing oscillator is 200 to 3000 rpm to generate a heterobinuclear complex; wherein the molar ratio of the second metal ion contained in the mixed solution B to the copper element contained in the suspension A is 0.8 to 1.2:1;
[0012] Step 4: Pretreatment of the carrier: The porous carbon carrier is placed in the cavity of a magnetron microwave oven, the microwave source uses a high-emission cylinder as the cathode and a resonant cavity as the anode, and the microwave is transmitted to the porous carbon carrier in a cyclotron manner. The microwave frequency is 2450MHz, and the output power is 100-1000W. The porous carbon carrier is subjected to microwave treatment under the protection of an inert gas, the gas flow rate is 10-150ml / min, and the microwave treatment time is 2-60min to obtain a pretreated carrier;
[0013] Step 5: Completion of the catalyst: Add the pretreated carrier obtained in step 4 to the mixed solution containing the heterobinuclear complex obtained in step 3 for immersion, so that the mass ratio of copper element to porous carbon carrier is 0.09-0.3:1, first heat to 50-100°C and continue stirring for 2-8h, cool naturally to room temperature and then stand for 8-24h, take out and put in a vacuum oven to dry for 12-24h, the drying temperature is 50-150°C, and a heterobinuclear copper-based catalyst for vinyl chloride synthesis reaction is obtained.
[0014] Further, the copper salt in step 1 is one or more of cuprous chloride, cuprous sulfide, cuprous bromide, cuprous iodide, cuprous cyanide, copper tetraacetonitrile perchlorate, copper tetraacetonitrile hexafluorophosphate, copper tetraacetonitrile tetrafluoroborate, copper nitrate, copper sulfate, copper chloride, copper bromide, copper acetate, copper phosphate, copper pyrophosphate, copper perchlorate, copper ammonium chloride, and copper phthalocyanine.
[0015] Furthermore, the bridging ligand in step 1 is selected from one or more of nitrogen and / or sulfur heterocyclic compounds, Schiff base complexes, oxalamide complexes, and oxalate compounds. Furthermore, the bridging ligand is selected from one of the following: 4-vinylpyridine, 2-aminopyridine, 2,2'-bipyridine, 4,4'-dimethyl-2,2'-bipyridine, imidazole, 1,10-phenanthroline, 5-nitro-1,10-o-phenanthroline, 2,2',2"-triaminoethylamine, N,N'-bis(2-aminoethyl)oxamide, N,N'-bis(2-aminopropyl)oxamide, N,N'-(3-aminopropyl)oxamide, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, ammonium oxalate, 5-methylisophthalic acid, o-di[N,N'-di(2'-benzimidazolemethyl)amino]-trans-cyclohexane, methylpropyldiacid, iminodiacetic acid, and diethylenetriamine.
[0016] Furthermore, in step 1, the speed of the agitator is 500 to 1000 rpm, and the stirring time is 5 to 12 hours.
[0017] Furthermore, in step 1, the molar ratio of the copper element to the bridging ligand is 1:0.9-1.1.
[0018] Further, in step 2, the second metal salt is MX, wherein M represents a cation selected from one of potassium, magnesium, aluminum, chromium, manganese, iron, cobalt, nickel, zinc, gallium, zirconium, ruthenium, palladium, silver, cadmium, indium, tin, cesium, barium, and platinum; X represents an anion selected from SO4 2- 、NO3 - , Cl - ,I - Br - 、ClO4 - PO4 3- 、SO3 2- 、NO2 - 、ClO3 - 、CH3COO - One of them.
[0019] Furthermore, the anion of the ionic liquid in step 2 is selected from halogen ions (Cl - Br - ,I - ), one or more of trifluoromethanesulfonate ion, tetrafluoroborate ion, hexafluorophosphate ion, nitrate ion, hydrogen sulfate ion, thiocyanate ion, perchlorate ion, dinitrile amide ion, acetate ion, trifluoroacetate ion, phosphate ion, and dihydrogen phosphate ion; the cation is selected from one or more of quaternary ammonium cations, quaternary phosphonium salts, pyridinium salts, imidazolium salts, pyrrolidines, pyrrolidones, piperidines, morpholines, thiazoles, and guanidine cations.
[0020] Furthermore, the ionic liquid is selected from at least one of the ionic liquids represented by formula (I) to formula (V):
[0021]
[0022] In formula (I),
[0023] R1 is H, CH3 or C2H5;
[0024] R2 is C n H 2n+1 , where n is an integer and 0≤n≤14;
[0025] R3 is C k H 2k+1 , where k is an integer and 0≤k≤4;
[0026] X1 - is chloride, bromide, nitrate, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate;
[0027] Furthermore, the ionic liquid represented by formula (I) is selected from one of the following:
[0028] 1-Methyl-3-octylimidazolium hexafluorophosphate, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexyl-3-methylimidazolium nitrate, 1-butyl-3-methylimidazolium chloride;
[0029]
[0030] In formula (II),
[0031] R4, R5, R6, and R7 are each independently C m H 2m+1 or phenyl, wherein m is an integer and 0≤m≤6;
[0032] X2 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate;
[0033] Furthermore, the ionic liquid represented by formula (II) is selected from one of the following:
[0034] Tetrabutylphosphine hexafluorophosphate, tributylhexylphosphine tetrafluoroborate, tributylethylphosphine bromide, tributylmethylphosphine p-toluenesulfonate;
[0035]
[0036] In formula (III),
[0037] R8, R9, R 10 , R 11 Each is independent of C j H 2j+1 or C substituted by C1-C4 alkoxy or phenyl j H 2j+1 , where j is an integer and 1≤n≤18;
[0038] X3 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate;
[0039] Furthermore, the ionic liquid represented by formula (III) is selected from one of the following:
[0040] Tributylmethylammonium bis(trifluoromethanesulfonyl imide), N-methoxyethyl-N-methyl-N,N-diethylammonium tetrafluoroborate, benzyltrimethylammonium chloride, trihexylmethylammonium bis(trifluoromethanesulfonic acid)imide, octadecyltrimethylammonium chloride;
[0041]
[0042] In formula (IV),
[0043] R 12 , R 13 Each is independent of C p H 2p+1 , where p is an integer and 0≤n≤6;
[0044] R 14 C q H 2q+1 , sulfur or oxygen atom, wherein q is an integer and 0≤n≤6;
[0045] X4 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, trifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate;
[0046] Furthermore, the ionic liquid represented by formula (IV) is selected from one of the following:
[0047] N-butyl-N-methylpyrrolidone bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidone bromide, pyrrolidone hexafluorophosphate, N-ethyl-N-methylpyrrolidone tetrafluoroborate;
[0048]
[0049] In formula (V),
[0050] R 15 C r H 2r+1 , where r is an integer and 0≤n≤16;
[0051] X5 - It is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate.
[0052] Furthermore, the ionic liquid represented by formula (V) is preferably selected from the following:
[0053] N-octylpyridinium bromide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-methylpyridinium hexafluorophosphate, N-hexadecylpyridinium trifluoromethanesulfonate, N-butylpyridinium tetrafluoroborate.
[0054] Furthermore, the solvent A and the solvent B are each independently one or more of water, methanol, ethanol, acetonitrile, acetone, toluene, DMF, tetrahydrofuran, methyl ether, and ethyl ether.
[0055] Furthermore, in step three, the rotation speed of the vortex mixing oscillator is 500 to 1000 rpm, and the continuous stirring time is 5 to 12 hours.
[0056] Furthermore, in step 4, the porous carbon carrier is activated carbon or mesoporous carbon, with a particle size of 10 to 100 meshes and a specific surface area of 100 to 1500 m 2 / g, pore volume 0.25~1.5ml 3 / g.
[0057] Furthermore, in step 4, the output power is 500-1000 W, the gas flow rate is 50-150 ml / min, and the time is 10-50 min.
[0058] Furthermore, in step five, the mass ratio of the copper element to the porous carbon carrier is controlled to be 0.09-0.15:1.
[0059] In a second aspect, the present invention provides a hetero-binuclear copper-based catalyst prepared according to the above preparation method. The active component of the catalyst belongs to a hetero-binuclear metal compound, and a copper atom and a second metal atom coexist in the molecule, and the two metal atoms are connected by a bridging ligand, and the other ends of the two metal atoms are connected to the terminal ligand to achieve the effect of limiting and regulating the structure type of the complex.
[0060] In a third aspect, the present invention provides the use of the hetero-binuclear copper-based catalyst in catalyzing the reaction of synthesizing vinyl chloride by acetylene hydrochlorination.
[0061] The application is specifically as follows: in a fixed bed reactor, the heterobinuclear copper-based catalyst is loaded, raw gas HCl and C2H2 are introduced, the reaction temperature is controlled at 100-240°C, the reaction pressure is controlled at 0.01-2MPa, and vinyl chloride is obtained by reaction.
[0062] Furthermore, the molar ratio of the raw gas is n(HCl):n(C2H2)=1:1-1.5:1, and the volumetric space velocity of acetylene is 10-500h -1 .
[0063] Compared with the prior art, the present invention has the following innovations and technical advantages:
[0064] (1) The present invention uses a vortex mixing oscillator in the synthesis process of the heterobinuclear complex, and utilizes the principle of eccentric rotation to generate a vortex in the liquid in the container, so that the two mononuclear complexes can be fully and quickly mixed and coordinated, forming more stable binuclear complexes and shortening the coordination time.
[0065] (2) The present invention uses an inert gas microwave-assisted treatment method for the pretreatment of the carrier. After the microwave treatment, the carrier can effectively remove other impurities in the carrier, improve the stability of the carrier, and prevent the metal particles from sintering within a certain temperature range, making the metal active components more dispersed, thereby improving the activity and stability of the catalyst.
[0066] (2) The catalyst prepared by the present invention is a heterobinuclear copper-based catalyst, which has more than twice the metal active centers compared with traditional catalysts and mononuclear ligand catalysts. Ionic liquids are green solvents composed entirely of anions and cations, and do not contain electrically neutral molecules. They can provide a large number of ligands, and the coordination structure with them as end groups is more stable and controllable, which greatly improves the activity and stability of the catalyst. Compared with single metal core catalysts, heterobinuclear catalysts can utilize the synergistic effect of different metals on copper to exert superior performance beyond that of a single element, thereby making it difficult for active components to be lost, further improving the activity and stability of the catalyst. Therefore, the catalyst is applied to the vinyl chloride synthesis reaction, showing ultra-long stability and ultra-high activity, and has good economic applicability and industrial application value. DETAILED DESCRIPTION
[0067] The present invention is described below with specific examples. It is necessary to point out that the examples are only used to further illustrate the present invention, but cannot be understood as limiting the scope of protection of the present invention, and the present invention is not limited thereto in any way. Those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.
[0068] Example 1
[0069] (1) 11.5 g of copper chloride and 16.2 g of N,N'-bis(2-aminoethyl)oxalamide were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0070] (2) 10.4 g of zinc chloride and 13.64 g of 1-butyl-3-methylimidazolium chloride were dissolved in 100 ml of acetone and mixed in a magnetic stirrer for 8 h at a speed of 600 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0071] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and stirring for 6 h at a vortex mixer speed of 800 rpm;
[0072] (4) In a 100 ml / min N2 atmosphere, columnar activated carbon (particle size 20 mesh, specific surface area 1217 m 2 / g, pore volume is 0.69ml 3 / g, the same below) was placed in a magnetron microwave oven for microwave treatment, the activated carbon particle size was 20 mesh, the microwave frequency was 2450MHz, the output power was 800W, and it was taken out after treatment for 30 minutes for use;
[0073] (5) Take 50 g of the activated carbon treated in step (4) and add it to the mixed solution of step (3) for immersion, heat it to 60°C, continue stirring for 4 hours, cool it naturally to room temperature and let it stand for 8 hours, then put it in a vacuum oven at 120°C and dry it for 12 hours to obtain a Cu(Ⅱ)Zn(Ⅱ) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0074] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 160° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 30 h -1 , the catalyst activity was 99.5%, and the activity began to decrease slightly after running for 600 h.
[0075] Example 2
[0076] (1) Take 20 g of copper perchlorate and 15.5 g of 4,4'-diaminodiphenylmethane, dissolve them in 100 ml of acetonitrile and stir them in a magnetic stirrer for 6 h at a speed of 700 rpm;
[0077] (2) 11 g of cobalt chloride and 14.5 g of benzyltrimethylammonium chloride were dissolved in 100 ml of ether and mixed and placed in a magnetic stirrer for stirring for 6 h at a speed of 700 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0078] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and stirring continuously for 5 h at a vortex mixer speed of 600 rpm;
[0079] (4) In an N2 atmosphere of 80 ml / min, spherical activated carbon (particle size 20 mesh, specific surface area 834 m 2 / g, pore volume is 0.72ml 3 / g, the same below) was placed in a magnetron microwave oven cavity for microwave treatment, the microwave frequency was 2450MHz, the output power was 600W, and after 20min of treatment, it was taken out for use;
[0080] (5) 50 g of the spherical activated carbon treated in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 70° C., stirring was continued for 3 h, the mixture was naturally cooled to room temperature and then allowed to stand for 7 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Co(II) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0081] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 170° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 50 h -1 , the catalyst activity was 99.2%, and the activity began to decrease slightly after running for 500 h.
[0082] Example 3
[0083] (1) 14.6 g of copper nitrate and 8.2 g of 4-vinylpyridine were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 7 h at a speed of 900 rpm;
[0084] (2) 15.6 g of nickel nitrate and 14.1 g of pyrrolidone hexafluorophosphate were dissolved in 100 ml of ethanol and mixed in a magnetic stirrer for 7 h at a speed of 900 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0085] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and continuously stirring for 6 h at a vortex mixer speed of 700 rpm;
[0086] (4) In a 60 ml / min N2 atmosphere, activated carbon flakes (particle size 20 mesh, specific surface area 1087 m 2 / g, pore volume is 0.89ml 3 / g, the same below) was placed in a magnetron microwave oven cavity for microwave treatment, the microwave frequency was 2450MHz, the output power was 700W, and after 25min of treatment, it was taken out for use;
[0087] (5) 50 g of the activated carbon flakes treated in step (4) were added to the mixed solution of step (3) for immersion, the temperature was raised to 50° C., stirring was continued for 5 h, the mixture was naturally cooled to room temperature and then allowed to stand for 8 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Ni(II) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0088] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 180° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 100 h -1 , the catalyst activity was 98.9%, and the activity began to decrease slightly after running for 500 h.
[0089] Example 4
[0090] (1) Take 10 g of copper phosphate and 11.4 g of 2,2',2"-triaminoethylamine, dissolve them in 100 ml of DMF and mix them in a magnetic stirrer for 8 h at a speed of 800 rpm;
[0091] (2) 14.5 g of ferric chloride and 17.4 g of N-butylpyridinium tetrafluoroborate were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 800 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0092] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and continuously stirring for 8 h at a vortex mixer speed of 800 rpm;
[0093] (4) In a 120 ml / min N2 atmosphere, the columnar activated carbon was placed in a magnetron microwave oven cavity for microwave treatment at a microwave frequency of 2450 MHz and an output power of 800 W. After the treatment for 40 min, the activated carbon was taken out for use;
[0094] (5) 50 g of the activated carbon treated in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 70° C., stirring was continued for 4 h, the mixture was naturally cooled to room temperature and then allowed to stand for 8 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Fe(III) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0095] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 200° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 120 h -1 , the catalyst activity was 99.2%, and the activity began to decrease slightly after running for 400 h.
[0096] Example 5
[0097] (1) Take 17 g of tetraacetonitrile copper perchlorate and 14.7 g of tris(3-aminopropyl)amine, dissolve them in 100 ml of methanol, mix them and place them in a magnetic stirrer for stirring for 5 h at a speed of 1000 rpm;
[0098] (2) 6.6 g of silver chloride and 9 g of tributyl ethyl phosphonium bromide were dissolved in 100 ml of methyl ether, mixed and placed in a magnetic stirrer for stirring for 5 h at a speed of 1000 rpm, and allowed to stand for stratification. The lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times;
[0099] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and stirring continuously for 5 h at a vortex mixer speed of 1000 rpm;
[0100] (4) In an atmosphere of 80 ml / min N2, the spherical activated carbon was placed in a magnetron microwave oven cavity for microwave treatment at a microwave frequency of 2450 MHz and an output power of 800 W. After treatment for 15 min, the activated carbon was taken out for use;
[0101] (5) 50 g of the activated carbon treated in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 60° C., stirring was continued for 5 h, the mixture was naturally cooled to room temperature and then allowed to stand for 12 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(I)Ag(I) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0102] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 150° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 150 h -1, the catalyst activity was 98.8%, and the activity began to decrease slightly after running for 500 h.
[0103] Example 6
[0104] (1) Take 12.5 g of copper sulfate and 14 g of 5-methylisophthalic acid, dissolve them in 100 ml of acetonitrile and mix them in a magnetic stirrer for 12 h at a speed of 500 rpm;
[0105] (2) 25.6 g of chromium chloride and 11.4 g of 1-hexyl-3-methylimidazole nitrate were dissolved in 100 ml of acetone and placed in a magnetic stirrer for stirring for 12 h at a speed of 500 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times;
[0106] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and stirring continuously for 12 h at a vortex mixer speed of 500 rpm;
[0107] (4) In a N2 atmosphere at 120 ml / min, mesoporous carbon (particle size 30 mesh, specific surface area 1378 m 2 / g, pore volume is 0.87ml 3 / g) was placed in a magnetron microwave oven cavity for microwave treatment, with a microwave frequency of 2450MHz and an output power of 1000W, and taken out after treatment for 10 minutes for standby use;
[0108] (5) 50 g of the mesoporous carbon treated in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 60° C., stirring was continued for 6 h, the mixture was naturally cooled to room temperature and then allowed to stand for 8 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Cr(III) / OMC binuclear catalyst for acetylene hydrochlorination reaction.
[0109] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 140° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 200 h -1 , the catalyst activity was 99.1%, and the activity began to decrease slightly after running for 400 h.
[0110] Comparative Example 1
[0111] Comparative Example 1 is used to illustrate the role of the vortex mixing oscillator in the catalyst preparation process by comparison with Example 1.
[0112] (1) 11.5 g of copper chloride and 16.2 g of N,N'-bis(2-aminoethyl)oxalamide were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0113] (2) 10.4 g of zinc chloride and 13.64 g of 1-butyl-3-methylimidazolium chloride were dissolved in 100 ml of acetone and mixed in a magnetic stirrer for 8 h at a speed of 600 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0114] (3) placing the suspension obtained in step (1) into a stirrer, slowly adding the liquid obtained in step (2) thereto, and continuing stirring for 6 hours;
[0115] (4) In a 100 ml / min N2 atmosphere, the columnar activated carbon was placed in a magnetron microwave oven cavity for microwave treatment. The activated carbon particle size was 20 mesh, the microwave frequency was 2450 MHz, the output power was 800 W, and it was taken out after treatment for 30 min for use;
[0116] (5) 50 g of the activated carbon treated in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 60° C., stirring was continued for 4 h, the mixture was naturally cooled to room temperature and allowed to stand for 8 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Zn(II) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0117] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 160° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 30 h -1 The catalyst activity was 72.4%, and the activity began to decline after 300 h of operation.
[0118] Comparative Example 2
[0119] Comparative Example 2 is used to illustrate the effect of inert gas microwave treatment of the carrier in the catalyst preparation process by comparison with Example 1.
[0120] (1) 11.5 g of copper chloride and 16.2 g of N,N'-bis(2-aminoethyl)oxalamide were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0121] (2) 10.4 g of zinc chloride and 13.64 g of 1-butyl-3-methylimidazolium chloride were dissolved in 100 ml of acetone and mixed in a magnetic stirrer for 8 h at a speed of 600 rpm. The mixture was allowed to stand for stratification, and the lower layer of the solution was separated with a separatory funnel and washed with deionized water for more than three times.
[0122] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid obtained in step (2) thereto, and stirring for 6 h at a vortex mixer speed of 800 rpm;
[0123] (4) Prepare columnar activated carbon with a particle size of 20 mesh for standby use;
[0124] (5) 50 g of the activated carbon prepared in step (4) was added to the mixed solution of step (3) for immersion, the temperature was raised to 60° C., stirring was continued for 4 h, the mixture was naturally cooled to room temperature and then allowed to stand for 8 h, and then dried in a vacuum oven at 120° C. for 12 h to obtain a Cu(II)Zn(II) / AC binuclear catalyst for acetylene hydrochlorination reaction.
[0125] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 160° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 30 h -1 , the catalyst activity was 82.5%, and the activity began to decline after running for 250 hours.
[0126] Comparative Example 3
[0127] Comparative Example 3 is compared with Example 1 to illustrate the advantages of the heterobinuclear copper-based catalyst over the ordinary copper-based second metal promoter catalyst.
[0128] (1) 11.5 g of copper chloride and 10.4 g of zinc chloride were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0129] (2) In a 100 ml / min N2 atmosphere, the columnar activated carbon was placed in a magnetron microwave oven cavity for microwave treatment. The activated carbon particle size was 20 mesh, the microwave frequency was 2450 MHz, the output power was 800 W, and it was taken out after treatment for 30 min for use;
[0130] (3) Take 50 g of the activated carbon treated in step (2) and add it to the mixed solution of step (1) for impregnation. After standing for 12 hours, put it in a vacuum oven at 120° C. and dry it for 12 hours to obtain a Cu-Zn / AC catalyst for acetylene hydrochlorination reaction.
[0131] (4) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 160° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 30 h -1 The catalyst activity was 34.8%, and the activity began to decline after running for 50 hours.
[0132] Comparative Example 4
[0133] Comparative Example 4 is compared with Example 1 to illustrate the advantages of the heterobinuclear catalyst compared with the catalyst with a single metal core.
[0134] (1) 11.5 g of copper chloride and 16.2 g of N,N'-bis(2-aminoethyl)oxalamide were dissolved in 100 ml of methanol and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0135] (2) 13.64 g of 1-butyl-3-methylimidazolium chloride was dissolved in 100 ml of acetone and placed in a magnetic stirrer for stirring for 8 h at a speed of 600 rpm;
[0136] (3) placing the suspension obtained in step (1) into a vortex mixer, slowly adding the liquid in step (2) thereto, and stirring continuously for 6 h at a vortex mixer speed of 800 rpm;
[0137] (4) In a 100 ml / min N2 atmosphere, the columnar activated carbon was placed in a magnetron microwave oven cavity for microwave treatment. The activated carbon particle size was 20 mesh, the microwave frequency was 2450 MHz, the output power was 800 W, and it was taken out after treatment for 30 min for use;
[0138] (5) Take 50 g of the activated carbon treated in step (4) and add it to the mixed solution of step (3) for immersion, heat it to 60°C, continue stirring for 4 hours, cool it naturally to room temperature and let it stand for 8 hours, then put it in a vacuum oven at 120°C and dry it for 12 hours to obtain a Cu / AC mononuclear catalyst for comparison.
[0139] (6) Then, 10 g of the catalyst was used for acetylene hydrochlorination in a fixed bed reactor. The reaction conditions were set as follows: temperature 160° C., reaction pressure 0.01 MPa, n(HCl):n(C2H2)=1.2:1, acetylene space velocity 30 h -1 , the catalyst activity was 67.4%, and the activity began to decline after running for 100 h.
Claims
1. A method for preparing a heterobinuclear copper-based catalyst for synthesizing vinyl chloride, characterized in that: The preparation method comprises the following steps: Step 1: Mix the copper salt, the bridging ligand and the solvent A and stir them in a magnetic stirrer at a speed of 100 to 2000 rpm for 2 to 24 hours to form a suspension A; the molar ratio of the copper element contained in the copper salt to the bridging ligand is 1:0.9 to 2; the feed ratio of the bridging ligand to the solvent A is 5 to 20 g:100 mL; the copper salt is selected from at least one of a monovalent copper salt and a divalent copper salt; Step 2: Mix the second metal salt, the ionic liquid as the terminal ligand and the solvent B and put them into a magnetic stirrer for stirring reaction, the stirrer speed is 200-2000rpm, the stirring time is 2-24h, then stand for stratification, separate the lower layer of liquid with a separatory funnel, and then repeatedly wash with deionized water for more than three times to obtain a mixed solution B; wherein the molar ratio of the ionic liquid to the second metal ion contained in the second metal salt is 1:0.9-2; the feed ratio of the ionic liquid to the solvent B is 7-20g:100ml; the second metal is selected from potassium, magnesium, aluminum, chromium, manganese, iron, cobalt, nickel, zinc, gallium, zirconium, ruthenium, palladium, silver, cadmium, indium, tin, cesium, barium, platinum; Step 3: Synthesis of heterobinuclear complex: Place the suspension A obtained in step 1 into a vortex mixer, and slowly add the mixed solution B obtained in step 2 into the suspension. The stirring is continued for 2 to 24 hours, and the rotation speed of the vortex mixing oscillator is 200 to 3000 rpm to generate a heterobinuclear complex; wherein the molar ratio of the second metal ion contained in the mixed solution B to the copper element contained in the suspension A is 0.8 to 1.2:1; Step 4: placing the porous carbon carrier into the cavity of a magnetron microwave oven, the microwave source uses a high-emission cylinder as the cathode and a resonant cavity as the anode, and the microwave is transmitted to the porous carbon carrier in a cyclotron manner. The microwave frequency is 2450 MHz, the output power is 100 to 1000 W, and the porous carbon carrier is subjected to microwave treatment under the protection of an inert gas, the gas flow rate is 10 to 150 ml / min, and the microwave treatment time is 2 to 60 min to obtain a pretreated carrier; Step 5: Add the pretreated carrier obtained in step 4 to the mixed solution containing the heterobinuclear complex obtained in step 3 for immersion, so that the mass ratio of copper element to porous carbon carrier is 0.09-0.3:1, first heat to 50-100°C and continue stirring for 2-8h, naturally cool to room temperature and then stand for 8-24h, take out and put in a vacuum oven to dry for 12-24h, the drying temperature is 50-150°C, and obtain a heterobinuclear copper-based catalyst for vinyl chloride synthesis reaction.
2. The preparation method according to claim 1, characterized in that: The copper salt is one or more of cuprous chloride, cuprous sulfide, cuprous bromide, cuprous iodide, cuprous cyanide, copper tetraacetonitrile perchlorate, copper tetraacetonitrile hexafluorophosphate, copper tetraacetonitrile tetrafluoroborate, copper nitrate, copper sulfate, copper chloride, copper bromide, copper acetate, copper phosphate, copper pyrophosphate, copper perchlorate, copper ammonium chloride, and copper phthalocyanine; The bridging ligand is selected from one or more of nitrogen and / or sulfur heterocyclic compounds, Schiff base complexes, oxalamide complexes, and oxalate compounds; The second metal salt is MX, wherein M represents a cation selected from potassium, magnesium, aluminum, chromium, manganese, iron, cobalt, nickel, zinc, gallium, zirconium, ruthenium, palladium, silver, cadmium, indium, tin, cesium, barium, and platinum; X represents an anion selected from SO4 2- 、NO3 - , Cl - ,I - Br - 、ClO4 - PO4 3- 、SO3 2- 、NO2 - 、ClO3 - 、CH3COO - One of; The anions of the ionic liquid are selected from one or more of halogen ions, trifluoromethanesulfonate ions, tetrafluoroborate ions, hexafluorophosphate ions, nitrate ions, hydrogen sulfate ions, thiocyanate ions, perchlorate ions, dinitrile amide ions, acetate ions, trifluoroacetate ions, phosphate ions, and dihydrogen phosphate ions; the cations are selected from one or more of quaternary ammonium cations, quaternary phosphonium salts, pyridinium salts, imidazolium salts, pyrrolidines, pyrrolidones, piperidines, morpholines, thiazoles, and guanidine cations.
3. The preparation method according to claim 2, characterized in that: The bridging ligand is selected from one of the following: 4-vinylpyridine, 2-aminopyridine, 2,2'-bipyridine, 4,4'-dimethyl-2,2'-bipyridine, imidazole, 1,10-phenanthroline, 5-nitro-1,10-o-phenanthroline, 2,2',2"-triaminoethylamine, N,N'-bis(2-aminoethyl)oxamide, N,N'-bis(2-aminopropyl)oxamide, N,N'-(3-aminopropyl)oxamide, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, ammonium oxalate, 5-methylisophthalic acid, o-di[N,N'-di(2'-benzimidazolemethyl)amino]-trans-cyclohexane, methylpropyldiacid, iminodiacetic acid, and diethylenetriamine.
4. The preparation method according to claim 2, characterized in that: The ionic liquid is selected from at least one of the ionic liquids represented by formula (I) to formula (V): In formula (I), R1 is H, CH3 or C2H5; R2 is C n H 2n+1 , where n is an integer and 0≤n≤14; R3 is C k H 2k+1 , where k is an integer and 0≤k≤4; X1 - is chloride, bromide, nitrate, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate; In formula (II), R4, R5, R6, and R7 are each independently C m H 2m+1 or phenyl, wherein m is an integer and 0≤m≤6; X2 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate; In formula (III), R8, R9, R 10 , R 11 Each is independent of C j H 2j+1 or C substituted by C1-C4 alkoxy or phenyl j H 2j+1 , where j is an integer and 1≤n≤18; X3 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate; In formula (IV), R 12 , R 13 Each is independent of C p H 2p+1 , where p is an integer and 0≤n≤6; R 14 C q H 2q+1 , sulfur or oxygen atom, wherein q is an integer and 0≤n≤6; X4 - is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, trifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate; In formula (V), R 15 C r H 2r+1 , where r is an integer and 0≤n≤16; X5 - It is chloride, bromide, hexafluorophosphate, tetrafluorophosphate, bistrifluoromethanesulfonyl imide, tetrafluoroborate, imide, trifluoromethanesulfonate or p-toluenesulfonate.
5. The preparation method according to claim 4, characterized in that: The ionic liquid represented by formula (I) is selected from the following: 1-Methyl-3-octylimidazolium hexafluorophosphate, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-hexyl-3-methylimidazolium nitrate, 1-butyl-3-methylimidazolium chloride; The ionic liquid represented by formula (II) is selected from the following: Tetrabutylphosphine hexafluorophosphate, tributylhexylphosphine tetrafluoroborate, tributylethylphosphine bromide, tributylmethylphosphine p-toluenesulfonate; The ionic liquid represented by formula (III) is selected from the following: Tributylmethylammonium bis(trifluoromethanesulfonyl imide), N-methoxyethyl-N-methyl-N,N-diethylammonium tetrafluoroborate, benzyltrimethylammonium chloride, trihexylmethylammonium bis(trifluoromethanesulfonic acid)imide, octadecyltrimethylammonium chloride; The ionic liquid represented by formula (IV) is selected from the following: N-butyl-N-methylpyrrolidone bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidone bromide, pyrrolidone hexafluorophosphate, N-ethyl-N-methylpyrrolidone tetrafluoroborate; The ionic liquid represented by formula (V) is selected from the following: N-octylpyridinium bromide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-methylpyridinium hexafluorophosphate, N-hexadecylpyridinium trifluoromethanesulfonate, N-butylpyridinium tetrafluoroborate.
6. The preparation method according to claim 1, characterized in that: The solvent A and solvent B are independently one or more of water, methanol, ethanol, acetonitrile, acetone, toluene, DMF, tetrahydrofuran, methyl ether, and ethyl ether.
7. The preparation method according to claim 1, characterized in that: In step 4, the porous carbon carrier is activated carbon or mesoporous carbon with a particle size of 10 to 100 mesh and a specific surface area of 100 to 1500 m 2 / g, pore volume 0.25~1.5ml 3 / g.
8. A heterobinuclear copper-based catalyst prepared according to the preparation method of claim 1.
9. Use of the heterobinuclear copper-based catalyst as claimed in claim 8 in catalyzing the reaction of synthesizing vinyl chloride by acetylene hydrochlorination.
10. The use according to claim 9, characterized in that The application is specifically as follows: in a fixed bed reactor, the heterobinuclear copper-based catalyst is loaded, raw material gases HCl and C2H2 are introduced, the reaction temperature is controlled at 100-240°C, the reaction pressure is controlled at 0.01-2MPa, and vinyl chloride is obtained by reaction.
Citation Information
Patent Citations
Catalyst for acetylene hydrochlorination and preparation method and application thereof
CN110961112A
Alcohol-copper complex catalyst, preparation method thereof and application thereof in acetylene hydrochlorination reaction
CN111151299A
Copper-based catalyst for preparing vinyl chloride through acetylene hydro-chlorination and preparation and use method thereof
CN111715253A
Vinyl chloride preparation method and system thereof
CN107840779A
Preparation method and application of copper catalyst for acetylene hydrochlorination reaction
CN112642448A