A silica sol for chemical mechanical polishing and its preparation method and application
By using ethyl orthosilicate and water to prepare silica sol under alkaline catalysis, the problems of complex and poor environmental protection of existing silica sol preparation processes are solved, uniform particle size and high dispersion are achieved, and the efficiency of chemical mechanical polishing is improved. and environmentally friendly.
Patent Information
- Application Number
- CN202310106131.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-13
AI Technical Summary
The existing silicon sol preparation process is complex, the reaction time is long, and the uniformity is poor, which cannot meet the fine polishing requirements of chemical mechanical polishing, and the use of surfactants leads to poor environmental protection.
Using ethyl orthosilicate (TEOS) as the silicon source and water as the solvent, under the action of an alkaline catalyst, the particle size of silica is controlled between 10 and 100 nm by controlling the aqueous phase pH, reaction temperature and stirring speed, and the silicon dioxide particle size is controlled between 10 and 100 nm to prepare A uniform and dispersible silica sol is produced for chemical mechanical polishing.
It significantly improves the material removal rate, improves the surface quality of the workpiece, reduces scratches and scratches during polishing, reduces the surface roughness, and does not use surfactants, which improves environmental protection.
Smart Images

Figure HDA0004074894520000011 
Figure HDA0004074894520000012 
Figure HDA0004074894520000021
Abstract
Description
Technical Field
[0001] The invention relates to a silica sol for chemical mechanical polishing and a preparation method and application thereof, belonging to the technical field of nano materials. Background Art
[0002] Chemical mechanical polishing (CMP) is one of the most advanced planarization technologies and an essential polishing process in the semiconductor manufacturing process. The basic principle of the CMP process is that the polishing workpiece rotates relative to the polishing pad under a certain pressure and in the presence of a polishing liquid. During this process, the oxidant in the polishing liquid between the workpiece surface and the polishing pad reacts chemically with the workpiece surface material, producing a layer of chemical reaction film on the workpiece surface. This layer of chemical reaction film is then removed by the abrasive in the polishing liquid and the polishing pad through mechanical grinding, exposing the workpiece surface again. Finally, effective removal and good surface quality are achieved in the alternation of chemical reaction and mechanical grinding.
[0003] Under the condition that the polishing machine and the workpiece to be polished are already clear, the polishing liquid and polishing conditions become the main factors that have a greater impact on the polishing results, among which the polishing liquid is the decisive factor affecting the CMP performance. The polishing liquid is composed of abrasives, soluble chemicals (oxidants, pH adjusters, dispersants, etc.) and water media. Abrasives are the main components of the polishing liquid and directly affect the surface quality and material removal rate. Therefore, the hardness, particle size, morphology and uniformity of the abrasive have a great influence on the quality of the workpiece after CMP.
[0004] Commonly used abrasives in chemical mechanical polishing liquids are silicon dioxide, aluminum oxide, and cerium oxide. Aluminum oxide has a high hardness, is easy to agglomerate, and has poor dispersibility. It is usually used on some materials with higher hardness, such as silicon carbide. Cerium oxide has moderate hardness. Since cerium has multiple valence states and is easy to transform between different valence states, it is easy to oxidize or complex the glass surface material, so it is widely used in chemical mechanical polishing of mobile phone screens, optical glass, etc. Silica sol is a dispersion formed by nano-scale silica particles in water or solvent. Since silica sol has good dispersibility and stability, polishing liquid composed of silica sol has been widely used in semiconductor polishing.
[0005] Research has found that spherical silica polishing liquid with small and uniform particle size can reduce polishing scratches and better meet the requirements of CMP abrasives for high-quality wafer surfaces. The commonly used method for producing silica sol in industry is the ion exchange method. However, this method has a complex preparation process, a long reaction time, and poor uniformity of synthesized silica, which cannot meet the requirements of CMP fine polishing. In addition, the preparation of existing silica sol requires the addition of surfactants as templates and additives, otherwise the uniformity and stability of the resulting silica sol are poor. However, the use of surfactants leads to poor environmental protection of silica sol.
[0006] Therefore, a method for preparing a silica sol with a simple preparation process, short reaction time, uniform particle size distribution, small and uniform particle size, and environmental friendliness is needed to improve CMP abrasives. To this end, the present invention is proposed. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a silica sol for chemical mechanical polishing and a preparation method and application thereof. The method was improved by using tetraethyl orthosilicate (TEOS) as the silicon source and water as the solvent. Under the action of alkaline catalyst, TEOS slowly hydrolyzes at the oil-water interface and continuously provides silicate substances to the water phase. The silicate substances are immediately consumed for the growth of the mother particles without forming new particles. By controlling the pH of the water phase, the reaction temperature, the stirring speed of the reaction liquid and the quality of TEOS, the silica particle size can be effectively controlled between 10 and 100 nm, and a silica sol with uniform particle size and good dispersibility can be obtained. It can be used in the fine polishing of CMP, which can significantly increase the material removal rate and improve the surface quality of the workpiece.
[0008] In order to achieve the above technical objectives, the present invention is specifically implemented through the following technical solutions:
[0009] A method for preparing silica sol for chemical mechanical polishing comprises the following steps:
[0010] An alkaline catalyst is added into water to obtain a mixed solution, and then the mixed solution is heated to a reaction temperature, and tetraethyl orthosilicate (TEOS) is added to react under stirring conditions; after the reaction is completed, a silica sol for chemical mechanical polishing is obtained.
[0011] Preferably according to the present invention, the alkaline catalyst is a Tris-HCl buffer or an ammonia-ammonium chloride buffer; further preferably an ammonia-ammonium chloride buffer; the pH value of the Tris-HCl buffer is 8-9, the pH value of the ammonia-ammonium chloride buffer is 10-11, and the mass fraction of ammonia in the ammonia water is 25-28wt%.
[0012] According to the preferred embodiment of the present invention, the pH value of the mixed solution is 8 to 11, and more preferably 9 to 10.5.
[0013] According to the present invention, preferably, the reaction temperature is 25-100°C, more preferably 40-80°C.
[0014] Preferably, according to the present invention, the mass ratio of tetraethyl orthosilicate (TEOS) to water is 0.1-1:1; the tetraethyl orthosilicate (TEOS) is added to the system in 2-6 batches, and each batch of tetraethyl orthosilicate is stirred and reacted for 2-8 hours.
[0015] Preferably according to the present invention, the stirring speed is 200-2000 rpm.
[0016] Preferably according to the present invention, the solid content of silicon dioxide in the obtained silica sol for chemical mechanical polishing is 1-15 wt %, the pH value is 8-10, and the silicon dioxide particles are uniformly spherical with a particle size of 10-100 nm.
[0017] The invention also provides a silica sol for chemical mechanical polishing, which is prepared by the above preparation method.
[0018] According to the present invention, the above-mentioned silica sol for chemical mechanical polishing is used in a chemical mechanical polishing liquid; preferably, the silica sol for chemical mechanical polishing is used as an abrasive in a chemical polishing liquid for semiconductor materials and devices.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The silica sol for chemical mechanical polishing of the present invention uses tetraethyl orthosilicate (TEOS) as a silicon source and water as a solvent. Under the action of a specific alkaline catalyst of the present invention, by adjusting the pH of the aqueous phase, the rapid decrease in pH caused by TEOS hydrolysis can be overcome, and the polycondensation after TEOS hydrolysis can be promoted to form uniform nanoparticles. By controlling the reaction temperature, stirring speed, and the quality of the silicon source, the gradient particle size of silicon dioxide can be effectively regulated to 10 to 100 nm. The final synthesized silicon dioxide particle size is uniform and has good dispersibility. The silica sol has good stability and can be stored for a long time without sedimentation. At the same time, the silicon dioxide particles have a large surface area, which can increase the contact area between the workpiece and the abrasive in the polishing liquid, effectively improve the material removal rate, reduce scratches and scratches during the polishing process, and reduce the roughness of the surface of the polished workpiece.
[0021] 2. The preparation method of the silica sol of the present invention, Compared with the method, the present invention does not use a co-solvent, TEOS forms a two-phase interface after contacting with water, the oil phase and the water phase are brought into contact with each other by stirring, and a TEOS hydrolysis reaction occurs at the oil-water interface. The preparation process is simple to operate and easy to repeat. By controlling the reaction conditions, silicon dioxide with a particle size of 10 to 100 nm can be synthesized, which overcomes the technical difficulty of the prior art that silicon dioxide with different gradient particle sizes can only be prepared through a multi-step method.
[0022] 3. Compared with the reported literature and patents, the preparation method of the silica sol of the present invention uses only water as a solvent in the reaction system, and does not need to use a surfactant as a template and additive. The obtained silica sol is environmentally friendly, pollution-free, and has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a TEM image of the silica sol for chemical mechanical polishing prepared in Example 1.
[0024] Figure 2 This is a TEM image of the silica sol for chemical mechanical polishing prepared in Example 2.
[0025] Figure 3 The particle size distribution curves of the initial silica sol prepared in Example 2 and the silica sol before and after standing for six months.
[0026] Figure 4 This is a TEM image of the silica sol for chemical mechanical polishing prepared in Example 3.
[0027] Figure 5 The graph is a relationship between the change in film thickness and time after polishing the silicon dioxide film with the chemical mechanical polishing silica sol and PL-3 silica sol prepared in Examples 2 and 3.
[0028] Figure 6 This is an AFM image of the chemical mechanical polishing method obtained in Example 3 after polishing using silica sol as a polishing liquid abrasive. DETAILED DESCRIPTION
[0029] The present invention is further described below with reference to specific embodiments, but is not limited thereto.
[0030] Meanwhile, the experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0031] The PL-3 sol used in this experiment was purchased from Qingdao Fuso Refining Processing Co., Ltd.; the rough polishing liquid was VK-SP30W purchased from Hangzhou Zhitai Purification Technology Co., Ltd.
[0032] The mass fraction of ammonia (NH3) in the ammonia water used in the embodiment is 25-28wt%.
[0033] Example 1
[0034] A method for preparing silica sol for chemical mechanical polishing comprises the following steps:
[0035] Dissolve 1.08g of ammonium chloride in 4g of deionized water, add 6mL of ammonia water after complete dissolution, and then dilute to 20mL with deionized water. After ultrasonic mixing, an ammonia-ammonium chloride buffer solution with a pH value of 10.5 can be obtained. Take 1mL of ammonia-ammonium chloride buffer solution and add it to 82.67g of deionized water, stir and mix thoroughly to obtain a mixed solution with a pH value of 10.3. Heat the mixed solution to 50°C under oil bath conditions, adjust the speed to 640rpm, add 17.33g of TEOS, and the system becomes clear and transparent after 6h of reaction; continue to keep the temperature and stirring speed unchanged, add 17.33g of TEOS to the system, react for 6h, add 17.33g of TEOS, react for 6h, and finally add 17.33g of TEOS. After 6h of reaction, a light blue transparent spherical silica sol is obtained, which is a silica sol for chemical mechanical polishing, wherein the SiO2 solid content is 13.1wt%, and the pH is between 8 and 9.
[0036] The TEM image of the silica sol for chemical mechanical polishing prepared in this embodiment is as follows: Figure 1 As shown by Figure 1 It can be seen that the particle size of SiO2 in the obtained silica sol is about 20nm, with regular spherical shape, uniform particle size and good dispersibility.
[0037] Example 2
[0038] A method for preparing silica sol for chemical mechanical polishing comprises the following steps:
[0039] Dissolve 1.08g of ammonium chloride in 4g of deionized water, add 6mL of ammonia water after complete dissolution, and then dilute to 20mL with deionized water. After ultrasonic mixing, an ammonia-ammonium chloride buffer solution with a pH value of 10.5 can be obtained. Take 1mL of ammonia-ammonium chloride buffer solution and add it to 82.67g of deionized water, stir and mix thoroughly to obtain a mixed solution with a pH value of 10.3. Heat the mixed solution to 80°C under oil bath conditions, adjust the speed to 640rpm, add 17.33g of TEOS, and the system becomes clear and transparent after 4h of reaction; continue to keep the temperature and stirring speed unchanged, add 17.33g of TEOS to the system, react for 4h, then add 17.33g of TEOS, react for 4h, and finally add 17.33g of TEOS. After 4h of reaction, a light blue transparent spherical silica sol is obtained, which is a silica sol for chemical mechanical polishing, wherein the SiO2 solid content is 13.1wt%, and the pH is between 8 and 9.
[0040] The TEM image of the silica sol for chemical mechanical polishing prepared in this embodiment is as follows: Figure 2 As shown by Figure 2 It can be seen that the particle size of SiO2 in the obtained silica sol is about 30nm, with regular spherical shape, uniform particle size and good dispersibility.
[0041] The silica sol prepared in this example was subjected to stability analysis. The particle size distribution curves of the silica sol before and after standing for six months are shown in FIG. Figure 3 As shown by Figure 3 It can be seen that the particle size of the obtained silica sol remains basically unchanged after being left to stand for six months, indicating that the silica sol prepared in this example has good stability.
[0042] Example 3
[0043] A method for preparing silica sol for chemical mechanical polishing comprises the following steps:
[0044] Dissolve 1.08g of ammonium chloride in 4g of deionized water, add 6mL of ammonia water after complete dissolution, and then dilute to 20mL with deionized water. After ultrasonic mixing, an ammonia-ammonium chloride buffer solution with a pH value of 10.5 can be obtained. Take 1mL of ammonia-ammonium chloride buffer solution and add it to 82.67g of deionized water, stir and mix thoroughly to obtain a mixed solution with a pH of 10.3. Heat the mixed solution to 80°C under oil bath conditions, adjust the speed to 320rpm, add 17.33g of TEOS, and the system becomes clear and transparent after 6h of reaction; continue to keep the temperature and stirring speed unchanged, add 17.33g of TEOS to the system, react for 6h, add 17.33g of TEOS, react for 6h, and finally add 17.33g of TEOS. After 6h of reaction, a light blue transparent spherical silica sol is obtained, which is a silica sol for chemical mechanical polishing, wherein the SiO2 solid content is 13.1wt%, and the pH is between 8 and 9.
[0045] The TEM image of the silica sol for chemical mechanical polishing prepared in this embodiment is as follows: Figure 4 As shown by Figure 4 It can be seen that the particle size of SiO2 in the obtained silica sol is about 40nm, with regular spherical shape, uniform particle size and good dispersibility.
[0046] Comparative Example 1
[0047] A method for preparing a silica sol for chemical mechanical polishing is as described in Example 2, except that ammonia water is used as an alkaline catalyst, and the specific steps are: taking ammonia water and adding it to 82.67g of deionized water, stirring and mixing it thoroughly, and obtaining a mixed solution with a pH of 10.3. The mixed solution is heated to 80°C under oil bath conditions, the rotation speed is adjusted to 640rpm, 17.33g of TEOS is added, and after reacting for 2h, part of the oil phase TEOS in the upper layer is not reacted, and the pH of the system drops rapidly to about 8, and the silica sol cannot be obtained. Using a buffer solution to maintain the pH of the system within a certain range is a key condition for the present invention to be able to prepare a stable silica sol with uniform particle size.
[0048] Experimental Example 1 Effect of Chemical Mechanical Polishing of Silicon Dioxide on Silicon Dioxide Thin Film on Single Crystal Silicon Wafer
[0049] 1. Test materials: silica sol prepared in Examples 2 and 3 and PL-3 silica sol.
[0050] 2. Test method: Take the silica sol of Examples 2 and 3 of the present invention and PL-3 silica sol, dilute the PL-3 silica sol with water to the same solid content of 13.1wt% as that of Examples 2 and 3, stir and mix them evenly, and then perform chemical mechanical polishing test: Cut a 4-inch diameter single crystal silicon wafer with a 300nm silicon dioxide film deposited into 1*1cm 2 Take 8 samples and stick them evenly around the circumference of the carrier plate. Use UNIPOL-1200S automatic grinding and polishing machine for polishing test. The process parameters are as follows: polishing liquid flow rate 350mL / h, polishing pressure 36.75kPa, rotation speed 20rpm, polishing time 1, 2, 3, 4, 5min, and the polishing pad is the frosted leather polishing pad supporting the above-mentioned polishing machine.
[0051] Polishing rate detection method: The polishing rate is measured by a film thickness meter. The average thickness difference of 8 silicon wafers before and after polishing is measured, and a curve of the relationship between film thickness change and time is made.
[0052] 3. Test results: The relationship between the thickness change of the silica film after polishing and the time of the silica sol prepared in Examples 2 and 3 and PL-3 silica sol is as follows: Figure 5 As shown by Figure 5 It can be seen that the silica sol prepared in Examples 2 and 3 of the present invention has a better polishing effect on silicon dioxide film polishing than the purchased PL-3 silica sol.
[0053] Experimental Example 2 Effect of Silicon Dioxide on Chemical Mechanical Polishing of Single Crystal Silicon Wafers
[0054] 1. Test material: silica sol prepared in Example 3.
[0055] 2. Test methods:
[0056] (1) Preparation of fine polishing liquid: In parts by weight, 83.3 parts of the silica sol prepared in Example 3 of the present invention and 16.6 parts of oxidant hydrogen peroxide are taken, mixed and stirred evenly, and a polishing test is performed.
[0057] (2) Chemical mechanical polishing test: A 4-inch diameter single crystal silicon wafer was cut into 1*1 cm 2 Take 8 samples and paste them evenly around the circumference of the carrier plate. Use UNIPOL-1200S automatic grinding and polishing machine for polishing test. The process parameters are as follows:
[0058] Rough polishing: VK-SP30W polishing liquid flow rate is 350mL / h, polishing pressure is 36.75kPa, rotation speed is 80rpm, polishing time is 0.5h, and the polishing pad is the polyurethane polishing pad supporting the above-mentioned polishing machine.
[0059] Fine polishing: The flow rate of the mixed liquid of silica sol prepared in Example 3 and oxidant hydrogen peroxide is 700 mL / h, the polishing pressure is 36.75 kPa, the rotation speed is 80 rpm, the polishing time is 1.5 h, and the polishing pad is the frosted leather polishing pad supporting the above-mentioned polishing machine.
[0060] After the above rough polishing and fine polishing, ethanol is used for ultrasonic cleaning for 20 to 30 minutes, and then blown dry with nitrogen.
[0061] (3) Testing methods for polishing rate and surface roughness:
[0062] The weight difference of 8 silicon wafers before and after polishing was measured by the weight method. The weight difference was divided by the density and then by the area to obtain the thickness, which was then divided by the time to obtain the material removal rate. The surface roughness of the silicon wafers was measured by atomic force microscopy.
[0063] 3. Test results: After polishing, the material removal rate of the silicon wafer was measured to be 8.19um / h, the surface roughness was 0.076nm, and the surface of the silicon wafer was smooth without residue or scratches. Figure 6 The AFM scanning result of the silicon wafer after polishing shows that the silica sol prepared in Example 3 of the present invention can be applied to the chemical mechanical polishing liquid, which effectively improves the material removal rate, and the surface roughness of the obtained silicon wafer can be lower than 0.1 nm, indicating that the silica sol prepared in the present invention can be applied to the field of ultra-precision processing of semiconductors.
[0064] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a silica sol for chemical mechanical polishing, comprising the following steps: An alkaline catalyst is added into water to obtain a mixed solution, and then the mixed solution is heated to a reaction temperature, and then ethyl orthosilicate is added to react under stirring conditions; after the reaction is completed, a silica sol for chemical mechanical polishing is obtained; The alkaline catalyst is a Tris-HCl buffer or an ammonia-ammonium chloride buffer; the pH value of the mixed solution is 9-10.5; the reaction temperature is 25-100° C.; the mass ratio of tetraethyl orthosilicate to water is 0.1-1:1; only water is used as a solvent in the reaction system, and no surfactant is used as a template or additive; The solid content of silicon dioxide in the obtained silica sol for chemical mechanical polishing is 1-15wt%, the pH value is 8-9, and the silicon dioxide particles are uniformly spherical with a particle size of 10-100nm.
2. The method for preparing the silica sol for chemical mechanical polishing according to claim 1, characterized in that: The reaction temperature is 40-80°C.
3. The method for preparing the silica sol for chemical mechanical polishing according to claim 1, characterized in that: The ethyl orthosilicate is added into the system in 2 to 6 equal batches, and each batch of ethyl orthosilicate is stirred and reacted for 2 to 8 hours after being added.
4. The method for preparing the silica sol for chemical mechanical polishing according to claim 1, characterized in that: The stirring speed is 200-2000 rpm.