A high-gloss polish
Through the combination of inorganic abrasive particles, organic fluorosilicon, acidic substances and alkaline substances, the softness and settlement problems of traditional polishing agents are solved, the gloss and scratch resistance of the polishing agent are improved, and the polishing effect and stability are achieved. It is suitable for a variety of stone surfaces and has no odor after burning.
Patent Information
- Application Number
- CN202210362025.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-07
AI Technical Summary
Traditional polishing agents contain waxy, which makes the polishing layer soft, not scratch-resistant, has a short service life, and the abrasive particles in the acidic slurry increase with the storage time, resulting in settlement and delamination, affecting the polishing quality.
Using the combination of inorganic abrasive particles, organic fluorosilicon, acidic substances, alkaline substances, surfactants and oxides, through the selection of specific proportions and particle sizes, organic acids and chain organic alkalis are added to form a weak acid system, which enhances the attachment. Focus and scratch resistance, and promote dispersion of substances by controlling the reaction temperature in stages to avoid precipitation.
It improves the gloss, scratch resistance and toughness of the polishing agent, extends storage time, reduces the generation of acid mist, significantly improves the polishing effect and product stability, and is suitable for a variety of stone surfaces, without any odor after burning.
Smart Images

Figure BDA0003584187560000061 
Figure HDA0003584187570000011 
Figure HDA0003584187570000012
Abstract
Description
Technical Field
[0001] The present invention relates to C09G1, and more particularly to a polishing agent with high gloss. Background Art
[0002] With the development of society, people pay more and more attention to the quality of life, and the requirements for daily necessities, hardware products, electronic products and other products have also been further improved. They not only hope that they have good functions, but also hope that they have good appearance. In the face of such a trend, polishing has become an indispensable step for many products. Polishing is to make the surface of the workpiece smooth by processing it. The polishing agent is a kind of reagent with polishing function acting on the surface of the object.
[0003] The polishing agents commonly used in the market are often used to polish marble tiles, terrazzo tiles, etc., and the traditional polishing agents contain waxy ingredients. Therefore, the polished tiles are not only soft and scratch-resistant due to the presence of wax, but also have a short service life. They are also fire-resistant and have odors when burned. In addition, the size of the abrasive particles in the acidic slurry of the traditional polishing agent will gradually increase with the extension of storage time and the effect of the chemical components in the slurry. When the particle size is greater than 120 nanometers, sedimentation and stratification will occur, which seriously affects the polishing quality and causes product failure.
[0004] Patent No. CN108624238B provides a durable wear-resistant floor polish and a preparation method thereof. By adding modified acrylic resin, the adhesion, impact resistance, stain resistance and flexibility of the polish coating are improved, and it has a good mildew-proof effect. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present invention provides a polishing agent with high gloss, characterized in that the raw materials of the polishing agent include inorganic abrasive particles, organic fluorine silicon, acidic substances, alkaline substances, surfactants, and oxides.
[0006] As a preferred technical solution of the present invention, the inorganic abrasive particles are selected from one or more of brown corundum abrasive, white corundum abrasive, black corundum abrasive and diamond abrasive.
[0007] Preferably, the particle size of the brown corundum abrasive is 30-80 mesh, the particle size of the white corundum abrasive is 40-100 mesh, and the particle size of the black corundum abrasive is 70-100 mesh.
[0008] Further preferably, the weight ratio of the brown corundum abrasive to the white corundum abrasive is (2-4):1.
[0009] As a preferred technical solution of the present invention, the organic fluorine silicon is selected from one or more of fluorine silicon-modified organic silicone resin, fluorine silicon resin, and epoxy-modified organic silicone resin.
[0010] As a preferred technical solution of the present invention, the acidic substance is an organic acid.
[0011] As a preferred technical solution of the present invention, the organic acid is selected from one or more of acetic acid, ethyl sulfonic acid, dodecylbenzene sulfonic acid, citric acid, and oxalic acid.
[0012] Organic fluorine silicon has low surface energy and self-polishing properties, but because of this, its adhesion after film formation is also relatively low, and it is very easy to be peeled off, and its polishing ability cannot be maximized. The applicant unexpectedly discovered in the experiment that adding a specific organic acid to the organic fluorine silicon system can not only improve the adhesion of the organic fluorine silicon system after film formation to a certain extent, but also improve the scratch resistance and make it less likely to produce scratches. This may be because the α-silicon-based carbon anion in the organic silicon removes silanol to obtain olefins under acidic conditions. Due to the weakly acidic system provided by this system, only part of the organic fluorine silicon molecules participate in the reaction. The obtained olefins not only do not reduce the surface energy of the organic fluorine silicon, but can synergize with the surfactants and oxides in the system to produce intermolecular effects, thereby enhancing the binding force and maximizing its own self-polishing ability. In addition, the binding force generated by the synergistic action of molecules in this system is not easily destroyed by external forces, which improves its scratch resistance. This combination effect is particularly significant when the weight ratio of organic silicon fluoride: acidic substance: surfactant: oxide is (15-30): (7-14): (2-6): (1-5), and the scratch resistance and adhesion effects are most significant.
[0013] As a preferred technical solution of the present invention, the alkaline substance is a chain organic base.
[0014] As a preferred technical solution of the present invention, the chain organic base is selected from one or more of triethylamine, 2,4-hexanediamine and diethylamine.
[0015] The applicant has found that by adding a chain organic base, the generation of acid mist during the processing can be further reduced. This may be because the organic base undergoes solvation in the system, and the positive charge is evenly dispersed, thus promoting the stability of the system to a certain extent and weakening the more violent reaction caused by the introduction of acidic substances.
[0016] As a preferred technical solution of the present invention, the surfactant is selected from one or more of sodium alkylbenzene sulfonate, sodium silicate and sodium borate.
[0017] The CAS number of sodium alkylbenzene sulfonate is 25155-30-0.
[0018] As a preferred technical solution of the present invention, the inorganic abrasive particles include 5-14 parts, organic fluorine silicon includes 15-30 parts, acidic substances include 7-14 parts, alkaline substances include 8-13 parts, surfactants include 2-6 parts, and oxides include 1-5 parts.
[0019] Preferably, the oxide is silicon oxide and / or aluminum oxide.
[0020] More preferably, the oxide is silicon oxide.
[0021] As a traditional matting agent, silicon oxide has a polishing effect, but the matting effect is relatively strong, and its addition to the system will cause the system to have a tendency to precipitate during storage. After a large number of experiments, the applicant found that adding a specific proportion of silicon oxide to the system can not only avoid this precipitation tendency, but also increase the glossiness of the polishing agent after it is applied to marble tiles. The applicant speculates that this may be due to the fact that a specific proportion of silicon oxide and other substances in the organic fluorine silicon system cooperate with each other to form a stable system, so that each substance is evenly dispersed in the system. In addition, the various substances in the system work together to achieve a good polishing system with physical polishing of organic fluorine silicon as the main and chemical polishing of silicon oxide as the auxiliary. This effect is especially effective when applied to marble tiles, and the effect is more significant, the glossiness is significantly improved, and the storage time is significantly extended.
[0022] Preferably, the raw materials of the polishing agent also include 25-40 parts of distilled water.
[0023] The second aspect of the present invention provides a method for preparing a polishing agent with high gloss, comprising the following steps: (1) mixing and heating; and (2) cooling.
[0024] Step (1) specifically comprises mixing inorganic abrasive particles, organic fluorine silicon and organic acid by weight, heating to 60-65° C., and keeping warm for 20-30 minutes to obtain mixture A; adding chain organic base, surfactant, oxide and distilled water by weight to mixture A, heating to 65-70° C., and keeping warm for 1-1.5 hours to obtain mixture B; step (2) specifically comprises naturally cooling mixture B to 25° C. to obtain a polishing agent.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) Organic acid replaces inorganic strong acid, providing a weak acid environment, which improves the adhesion and scratch resistance of the system while reducing the corrosiveness of the polishing agent and preventing the acid mist from causing harm to technicians.
[0027] (2) By selecting inorganic abrasive particles of a specific proportion and specific particle size, the mechanical strength such as toughness of the polishing agent is improved.
[0028] (3) Adding organic base can further alleviate the harm that may be caused by acid corrosion and make the reaction milder.
[0029] (4) By controlling the temperature during the reaction process in stages, the reaction can proceed smoothly while promoting the full dispersion of the substances in the system, which is beneficial to maintaining the fluidity of the polishing agent and also facilitates the long-term storage of the polishing agent.
[0030] (5) When the polishing agent is used on materials such as marble, artificial stone, granite, and ceramic tiles, it has good gloss and a significant mirror effect.
[0031] (6) It focuses light under illumination, which improves the problem of scattered light in tiles polished by traditional wax-containing polishing agents. It can be applied to marble crystal surfaces, granite crystal surfaces, ceramic tile crystal surfaces, artificial granite crystal surfaces, terrazzo crystal surfaces, microcrystalline stone crystal surfaces, quartz crystal surfaces, etc. It is especially suitable for mixed paving of multiple varieties of stone and ceramic tiles.
[0032] (7) There is no odor after burning, and the feeling of use is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the polishing effect diagram of Example 1. Figure 2 This is the polishing effect diagram of Example 2. DETAILED DESCRIPTION
[0034] Example
[0035] The raw materials for preparing the composition in the embodiment are all commercially available, wherein the brown corundum abrasive is purchased from Lingshou County Shifeng Mining Processing Plant, model zgy, and particle size 46 mesh, the white corundum abrasive is purchased from Henan Qiansheng Refractory Abrasive Co., Ltd., model W63, and particle size 60 mesh, the fluorosilicone resin is purchased from Guangzhou Kanglunxi Chemical Technology Co., Ltd., model KX-501, and the CAS number of sodium alkylbenzene sulfonate is 25155-30-0, which is sodium dodecylbenzene sulfonate.
[0036] Example 1
[0037] This example provides a polishing agent with high gloss, which comprises, by weight, 7 parts of inorganic abrasive particles, 22 parts of organic fluorine silicon (specifically fluorine silicon resin), 10 parts of acidic substance (specifically oxalic acid), 8 parts of alkaline substance (specifically chain organic base, the chain organic base is triethylamine), 4 parts of surfactant (specifically sodium alkylbenzene sulfonate), 2 parts of oxide (specifically silicon oxide), and 30 parts of distilled water.
[0038] In the inorganic abrasive particles, the weight ratio of brown corundum abrasive to white corundum abrasive is 3:1.
[0039] This example also provides a method for preparing a high-gloss polishing agent, comprising the following steps: (1) mixing and heating; and (2) cooling.
[0040] Step (1) specifically comprises mixing inorganic abrasive particles, organic fluorine silicon and organic acid in parts by weight, heating to 60° C., and keeping warm for 25 minutes to obtain mixture A; adding chain organic base, surfactant, oxide and distilled water in parts by weight to mixture A, heating to 65° C., and keeping warm for 1.2 hours to obtain mixture B; step (2) specifically comprises naturally cooling mixture B to 25° C. to obtain a polishing agent.
[0041] Example 2
[0042] This example provides a polishing agent with high gloss. The difference from Example 1 is that the inorganic abrasive particles are 5 parts, organic fluorosilicone (specifically fluorosilicone resin) is 20 parts, acidic substance (specifically oxalic acid) is 7 parts, alkaline substance (specifically chain organic base triethylamine) is 7 parts, surfactant (specifically sodium alkylbenzene sulfonate) is 5 parts, oxide (specifically silicon oxide) is 3 parts, and distilled water is 33 parts.
[0043] This example also provides a method for preparing a polishing agent with high gloss, which is the same as the preparation method in Example 1.
[0044] Example 3
[0045] This example provides a polishing agent with high gloss. The difference from Example 1 is that the inorganic abrasive particles are 14 parts, organic fluorine silicon (specifically fluorosilicone resin) is 35 parts, acidic substance (specifically oxalic acid) is 15 parts, alkaline substance (specifically chain organic base triethylamine) is 13 parts, surfactant (specifically sodium alkylbenzene sulfonate) is 4 parts, oxide (specifically silicon oxide) is 3 parts, and distilled water is 35 parts.
[0046] This example also provides a method for preparing a polishing agent with high gloss, which is the same as the preparation method in Example 1.
[0047] Example 4
[0048] This example provides a polishing agent with high gloss. The difference from Example 1 is that, by weight, the inorganic abrasive particles are 13 parts, organic fluorosilicone (specifically fluorosilicone resin) is 27 parts, acidic substance (specifically oxalic acid) is 9 parts, alkaline substance (specifically chain organic base triethylamine) is 11 parts, surfactant (specifically sodium alkylbenzene sulfonate) is 4 parts, oxide (specifically silicon oxide) is 3 parts, and distilled water is 26 parts.
[0049] In the inorganic abrasive particles, the weight ratio of brown corundum abrasive to white corundum abrasive is 7:1.
[0050] This example also provides a method for preparing a polishing agent with high gloss, which is the same as the preparation method in Example 1.
[0051] Example 5
[0052] This example provides a polishing agent with high gloss, which is the same as Example 1.
[0053] This example also provides a method for preparing a polishing agent with high gloss, which is different from Example 1 in that: step (1) specifically comprises mixing inorganic abrasive particles, organic fluorine silicon, organic acid, chain organic base, surfactant, oxide and distilled water in parts by weight, heating to 65° C., and keeping warm for 1 hour to obtain a mixture B.
[0054] Performance Test:
[0055] 1. Polishing degree: Take 50g of the polishing agent obtained in Example 1-5 and apply it on a 1m 3 The gloss meter was used to test the glossiness of the marble tiles. The results are shown in Table 1:
[0056] Table 1
[0057]
[0058]
[0059] 2. Light-gathering effect test: Take 50g of the polishing agent obtained in Example 1-2 and apply it on a surface of 1m 3 On the marble tiles, observe under the light. Figure 1 , Figure 2 As shown, the marble tiles of Examples 1-2 have good light-collecting effect.
[0060] 3. Scratch resistance test: 50 g of the polish obtained in Example 1-5 was applied with a brush on a surface of 1 m 3 The scratch resistance test was carried out on marble tiles according to ISO12137-1. The results are shown in Table 2:
[0061] Table 2
[0062] Example Scratch resistance 1 Scratch resistant 2 Scratch resistant 3 Not scratch resistant 4 Not scratch resistant 5 Not scratch resistant
[0063] 4. Stability test: After the polishing agent is placed at room temperature for one week, 50g of the polishing agent is applied with a brush on a surface of 1m 3 The gloss meter was used to test the glossiness of the marble tiles. The results are shown in Table 3:
[0064] Table 3
[0065] Example Glossiness 1 99 2 94.5 3 79 4 79 5 80
[0066] It can be seen that the polishing agent obtained in Example 1-2 has high gloss, good focusing effect, and good scratch resistance. After being placed at room temperature for one week, it is applied on marble tiles and the gloss does not decrease, and has a certain stability.
Claims
1. A polishing agent with high gloss, characterized in that: By weight, 5-14 parts of inorganic abrasive particles, 15-30 parts of organic fluorine silicon, 7-14 parts of acidic substances, 8-13 parts of alkaline substances, 2-6 parts of surfactants, and 1-5 parts of oxides; The inorganic abrasive particles are brown corundum abrasive and white corundum abrasive, the weight ratio of which is (2-4):1, the particle size of the brown corundum abrasive is 46 mesh, and the particle size of the white corundum abrasive is 60 mesh; The acidic substance is an organic acid, and the organic acid is selected from one or more of acetic acid, ethyl sulfonic acid, dodecylbenzene sulfonic acid, citric acid, and oxalic acid; The alkaline substance is a chain organic base, and the chain organic base is selected from one or more of triethylamine, 2,4-hexanediamine, and diethylamine; The surfactant is sodium alkylbenzene sulfonate; The organic fluorine silicon is fluorine silicon resin, model KX-501; The method for preparing the polishing agent with high glossiness comprises: (1) Inorganic abrasive particles, organic fluorine silicon and organic acid are mixed by weight, heated to 60-65° C., and kept warm for 20-30 minutes to obtain a mixture A; a chain organic base, a surfactant, an oxide and distilled water are added to the mixture A by weight, heated to 65-70° C., and kept warm for 1-1.5 hours to obtain a mixture B; (2) The mixture B was naturally cooled to 25° C. to obtain a polishing agent.
2. A method for preparing a polishing agent with high gloss according to claim 1, characterized in that: The following steps are involved: (1) Mixing and heating; (2) Cooling.