A pGaN gate GaN HEMT based on self-stopping etch and its fabrication method
By employing a self-stopping etching technique that inserts an AlN layer into the pGaN gate structure, the problem of difficult etching control was solved, enabling the fabrication of high-performance pGaN gate gallium nitride high electron mobility transistors and improving product yield and performance.
Patent Information
- Application Number
- CN202310016178.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-01-06
AI Technical Summary
In the existing technology, the etching of pGaN gate gallium nitride high electron mobility transistors is difficult to control precisely, resulting in low product yield and performance degradation. In particular, the threshold voltage of enhancement-mode devices is insufficient and cannot meet actual needs.
By employing a self-stop etching technique, an AlN layer is inserted into the pGaN gate structure. Utilizing the high etching selectivity between AlN and pGaN, self-stop etching is achieved, forming a pGaN/AlN/pGaN cap structure. This allows for precise control of the etching depth and avoids damage to the interface.
This led to the development of high-performance pGaN gate gallium nitride high electron mobility transistors with good device characteristic consistency, improving product yield and transistor performance.
Smart Images

Figure CN115938941B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to pGaN gate gallium nitride high electron mobility transistors, specifically to a pGaN gate gallium nitride high electron mobility transistor fabricated based on a self-stopping etching method, belonging to the field of semiconductor device technology. Background Technology
[0002] Gallium nitride high electron mobility transistors (GaN HEMTs) based on the two-dimensional electron gas (2DEG) conductive channel in AlGaN / GaN heterojunctions possess excellent characteristics such as low conduction loss and high switching frequency, and are considered strong contenders for next-generation semiconductor power devices. Conventional GaN HEMTs are depletion-mode devices. To improve circuit safety and simplify the design of power device gate drive circuits, enhancement-mode power devices are required. Among the various mainstream technologies for realizing enhancement-mode GaN power devices, pGaN-gate GaN HEMTs are currently the mainstream enhancement-mode device technology due to their comprehensive advantages in performance, cost, and process maturity, and have already achieved commercial application.
[0003] In the fabrication of pGaN gate gallium nitride high electron mobility transistors (HEMTs), the etching of the active regions between the gate and source, and between the gate and drain, significantly impacts the transistor's electrical performance and requires precise control. However, current pGaN gate structure fabrication primarily employs dry etching techniques based on chlorine-based plasma inductively coupled plasma (ICP) or reactive ion etching (RIE). These dry etching methods suffer from difficulty in controlling the etching rate and uneven etching depth, leading to reduced yields of pGaN gate GaN HEMT products. Furthermore, the dry etching process easily damages the GaN surface, causing transistor performance degradation. Therefore, developing a self-stopping etching technique suitable for pGaN gate gallium nitride high electron mobility transistors is of great significance.
[0004] MIT employed a combined fluorine-based dry etching method and TMAH wet etching to etch 22-nm n-GaN / 1.5-nm AlN / 3-nm Al... 0.15 Ga 0.75 Self-stop etching of n-GaN was achieved on the barrier layer structure of N[1]. Since AlF3 is non-volatile, there is a high fluorine-based etching selectivity between GaN and AlN. After the fluorine-based dry etching of the 22nm n-GaN layer, it stops on the surface of the AlN layer. Then, the surface of the AlN layer is oxidized and TMAH wet etched to achieve self-stop etching and to fabricate a device with good electrical characteristics. However, the threshold voltage of the fabricated enhanced GaN HEMT is very low, only +0.3V, which cannot meet the actual application requirements.
[0005] Chang Gung University etched a 60 nm pGaN layer by performing multiple N2O oxidation and HCl wet etching processes, and stopped the etching on the AlN surface [2]. In each cycle, N2O plasma oxidizes GaN to Ga2O3, and Ga2O3 is etched by HCl wet etching, which is repeated multiple times. Since the rate of HCl etching of Al2O3 is very slow, self-stop etching can be achieved on the AlN layer surface. However, the inserted AlN layer will enhance the piezoelectric polarization effect, resulting in a decrease in the threshold voltage of the device; and multiple wet etching processes will cause the shape of the gate pGaN layer to change.
[0006] There is an urgent need for a self-stopping etching technique that can precisely control the pGaN etching depth and effectively avoid damaging the pGaN / AlGaN interface, so as to achieve the goal of fabricating high-performance pGaN gate gallium nitride high electron mobility transistors with good device characteristic consistency.
[0007] References:
[0008] [1] B.Lu, M.Sun and T.Palacios, "An Etch-Stop Barrier Structure for GaNHigh-Electron-Mobility Transistors," in IEEE Electron Device Letters, vol.34, no.3, pp.369-371, March 2013, doi:10.1109 / LED.2012.2237374.
[0009] [2]H.-C.Chiu et al., "High Uniformity Normally-OFF p-GaN Gate HEMTUsing Self-Terminated Digital Etching Technique," in IEEE Transactions onElectron Devices, vol.65, no.11, pp.4820-4825, Nov.2018, doi:10.1109 / TED.2018.2871689. Summary of the Invention
[0010] The purpose of this invention is to provide a method for fabricating a pGaN gate gallium nitride high electron mobility transistor based on self-stopping etching, in order to solve the problems of low transistor product yield and transistor performance degradation caused by existing etching techniques.
[0011] The technical solution of the present invention is as follows:
[0012] A pGaN gate gallium nitride high electron mobility transistor (HNT) fabricated using a self-stopping etching method employs a specific wafer epitaxial structure. The key feature is the insertion of an AlN layer near the barrier layer in the pGaN gate cap layer, forming a pGaN / AlN / pGaN cap layer structure. During fabrication, the high etch selectivity between AlN and pGaN is utilized to achieve self-stopping etching of the AlN surface while etching the upper pGaN layer. Then, the AlN layer and the lower pGaN layer are etched, completing the uniform etching of the active region pGaN / AlN / pGaN cap layer structure, resulting in a high-performance pGaN gate gallium nitride HNT HNT transistor with good device characteristic consistency.
[0013] The specific structure of the aforementioned pGaN gate gallium nitride high electron mobility transistor includes a substrate, and a buffer layer, a channel layer, and a barrier layer stacked sequentially from bottom to top on the substrate. The source, drain, and cap layer structures are located on the barrier layer, and the gate is located on the cap layer structure. The cap layer structure is a pGaN / AlN / pGaN three-layer structure, wherein the lower layer is a first gate p-type GaN cap layer, the middle layer is an AlN insertion layer, and the upper layer is a second gate p-type GaN cap layer, with the gate located on the second gate p-type GaN cap layer. A passivation layer covers the source, gate, and drain.
[0014] In the above-mentioned pGaN gate gallium nitride high electron mobility transistor, preferably, the thickness of the first gate p-type GaN cap layer is 10-300 nm, the thickness of the AlN insertion layer is 0.5-5 nm, and the thickness of the second gate p-type GaN cap layer is 2-50 nm.
[0015] In the aforementioned pGaN gate gallium nitride high electron mobility transistor, the substrate can be a Si substrate, SiC substrate, sapphire substrate, GaN substrate, etc.; the buffer layer can be one or more of GaN, AlN, InGaN, AlGaN, InAlGaN, etc.; the channel layer can be GaN, InGaN, AlGaN, InAlGaN, etc.; the barrier layer can be one or more of GaN, AlN, AlGaN, InGaN, InAlGaN, etc.; and the passivation layer can be SiO2, Si3N4, etc.
[0016] This invention also provides a method for fabricating a pGaN gate gallium nitride high electron mobility transistor, comprising the following steps:
[0017] 1) A buffer layer, a channel layer, a barrier layer, a first gate p-type GaN cap layer, an AlN insertion layer, and a second gate p-type GaN cap layer are sequentially grown on the substrate.
[0018] 2) Inductively coupled plasma (ICP) etching technology is used to dry etch the second gate p-type GaN cap layer using fluorine (F) etching gas. Due to the high etching selectivity between AlN and pGaN, the etching interface stops precisely on the surface of the AlN insertion layer, achieving self-stopping.
[0019] 3) Etch the AlN insertion layer and the first gate p-type GaN cap layer to form a pGaN / AlN / pGaN cap layer structure;
[0020] 4) A passivation layer is grown on the barrier layer and cap layer structure;
[0021] 5) Etch the passivation layer on the barrier layer to form grooves for depositing the source and drain, and then deposit electrode metal to form the source and drain.
[0022] 6) Form device isolation;
[0023] 7) Etch the passivation layer on the cap layer structure to form a groove for depositing gate metal, and then grow the gate metal to form the gate.
[0024] In step 2) above, after the fluorine-based dry etching, the sample can be immersed in an alkaline solution to remove any fluorides that may be present on the AlN surface after etching.
[0025] The device isolation method in step 6) above can be to perform ion implantation in the passivation layer region on the side of the device to form a device isolation region. The implanted ions can be one or more combinations of F, N, B, Ar, Fe ions, etc., so that the passivation layer in this region and the barrier layer and channel layer below it form a device isolation region; or, the passivation layer region on the side of the device can be etched to remove the passivation layer in this region and the barrier layer and channel layer below it, so that the two-dimensional electron gas (2DEG) disappears.
[0026] Furthermore, variations in parameters such as length, thickness, and doping concentration in different regions of the aforementioned pGaN gate GaN HEMT device fall within the scope of this invention, depending on different design requirements and fabrication processes. It is worth noting that the focus of this invention is on a technique for achieving self-stopping etching of the pGaN layer in the active region of a pGaN gate gallium nitride high electron mobility transistor. It is understood that other structures and variations are possible without departing from the scope of this invention. Moreover, different examples, structures, and processes can be combined to achieve the same objective.
[0027] The beneficial effects of this invention are:
[0028] This invention provides a method for fabricating a pGaN gate gallium nitride high electron mobility transistor based on self-stopping etching. This method can precisely control the etching depth of the pGaN / AlN / pGaN cap structure in the active region of the pGaN gate GaN HEMT device, and can effectively avoid damaging the interface between the pGaN cap layer and the barrier layer, ultimately achieving the goal of fabricating a high-performance pGaN gate gallium nitride high electron mobility transistor with good device characteristic consistency. Attached Figure Description
[0029] Figure 1 This is the completed effect diagram of step 1) of Example 1.
[0030] Figure 2 This is the completed effect diagram of step 2) of Example 1.
[0031] Figure 3 This is the effect diagram after step 3) of Example 1.
[0032] Figure 4 This is the completed effect diagram of step 4) of Example 1.
[0033] Figure 5 This is the completed effect diagram of step 5) of Example 1.
[0034] Figure 6 This is the completed effect diagram of step 6) of Example 1.
[0035] Figure 7 This is the effect diagram after step 7) of Example 1.
[0036] Figure 8 This is the completed effect diagram of step 8) of Example 1.
[0037] Figure 9 This is a cross-sectional view of the pGaN gate gallium nitride high electron mobility transistor device prepared in Example 1.
[0038] Figure 10 This is the effect diagram after step 7) of Example 2.
[0039] Figure 11 This is a cross-sectional view of the pGaN gate gallium nitride high electron mobility transistor device prepared in Embodiment 2 of the present invention. Detailed Implementation
[0040] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0041] Example 1
[0042] The pGaN gate gallium nitride high electron mobility transistor device structure fabricated in this embodiment is as follows: Figure 9 As shown, it includes:
[0043] Substrate 1 can be made of Si substrate, SiC substrate, sapphire substrate, or GaN substrate;
[0044] A buffer layer 2, which can reduce device leakage current and increase breakdown voltage, is located on the substrate 1. Its material can be one or more of GaN, AlN, InGaN, AlGaN, InAlGaN, etc.
[0045] The channel layer 3, which provides an electronic conductive channel, is located on the buffer layer 2, and its material can be GaN, InGaN, AlGaN, InAlGaN, etc.
[0046] A barrier layer 4, which generates a two-dimensional electron gas through polarization effect, is located on the channel layer 3. Its material can be one or more of GaN, AlN, AlGaN, InGaN, InAlGaN, etc.
[0047] A gate p-GaN structure that depletes two-dimensional electron gas is located on barrier layer 4, including a stacked first gate p-type GaN cap layer 5a, an AlN insertion layer 6a, and a second gate p-type GaN cap layer 7a.
[0048] The passivation layers 8a, 8b, 8b' and 8c, which are used as passivation layers on the surface of pGaN gate gallium nitride high electron mobility transistors, are located on barrier layer 4 and can be made of materials such as SiO2 and Si3N4.
[0049] pGaN gate GaN HEMT source 9 is located on the barrier layer 4 and embedded in the groove formed between the passivation layers 8a and 8b;
[0050] pGaN gate GaN HEMT drain 10 is located on the barrier layer 4 and embedded in the groove formed between the passivation layers 8b' and 8c;
[0051] Fluorine ion implantation device isolation regions 11a and 11b, used for isolation between different pGaN gate GaN HEMT devices, are located in the passivation layers 8a and 8c and in the barrier layer 4 and the channel layer 3 below them.
[0052] The pGaN gate GaN HEMT gate 12 is located on the second gate p-type GaN cap layer 7a and is embedded in the groove formed between the passivation layers 8b and 8b'.
[0053] The preparation steps are as follows:
[0054] 1) A buffer layer 2, a channel layer 3, a barrier layer 4, a first gate p-type GaN cap layer 5, an AlN insertion layer 6, and a second gate p-type GaN cap layer 7 are sequentially epitaxially grown on substrate 1, as follows: Figure 1 As shown;
[0055] 2) Using inductively coupled plasma (ICP) etching technology, a fluorine (F)-containing etching gas is selected for dry etching of the second gate p-type GaN cap layer 7. Due to the high etching selectivity between AlN and pGaN, the etching interface stops precisely on the surface of the AlN insertion layer 6, achieving self-stopping. This results in the uniform formation of the second gate p-type GaN cap layer 7a of the pGaN gate GaNHEMT across the entire wafer. Figure 2 As shown; and you can choose to immerse the sample in an alkaline solution for an appropriate time, such as in a developer, to remove any fluorides that may be present on the AlN surface after etching.
[0056] Note: For the dry etching in step 2), photoresist or other suitable materials can be used as the etching mask, such as hard masks such as SiO2, Al2O3 and HfO2.
[0057] 3) Etch the AlN insertion layer 6 and the first gate p-type GaN cap layer 5 to form the AlN insertion layer 6a and the first gate p-type GaN cap layer 5a, as shown. Figure 3 As shown;
[0058] 4) A passivation layer 8 is grown on the barrier layer 4 and the second gate p-type GaN cap layer 7a, such as... Figure 4 As shown;
[0059] 5) Etch the passivation layer 8 to form grooves for depositing source and drain channels, dividing the passivation layer 8 into three parts 8a, 8b, and 8c, as shown. Figure 5 As shown;
[0060] 6) Electrode metal is deposited on the barrier layer 4 to form the source 9 and drain 10 of the pGaN gate GaN HEMT, as shown below. Figure 6 As shown;
[0061] 7) Fluorine ion implantation is used to form fluorine ion implantation isolation regions 11a and 11b between GaN HEMTs with different pGaN gates, such as... Figure 7 As shown;
[0062] 8) Etch the passivation layer 8b to form a groove for depositing the gate metal, dividing the passivation layer 8b into two parts 8b and 8b', as shown. Figure 8 As shown;
[0063] 9) A gate metal is grown on the second gate p-type GaN cap layer 7a to form the gate 12 of the pGaN gate GaN HEMT, resulting in... Figure 9 The pGaN gate gallium nitride high electron mobility transistor shown is an example.
[0064] Example 2
[0065] The pGaN gate gallium nitride high electron mobility transistor device structure fabricated in this embodiment is as follows: Figure 11 As shown, the method of device isolation in this embodiment differs from that in Embodiment 1. For example... Figure 10 As shown in step 7) of this embodiment, by etching the passivation layer region on the side of the pGaN gate GaN HEMT, the passivation layer in this region and the barrier layer and electron conduction channel layer below it are etched away, so that the two-dimensional electron gas (2DEG) disappears.
[0066] The other structures and effects are consistent with those of Example 1.
Claims
1. A method for fabricating a pGaN-gate gallium nitride high electron mobility transistor, characterized in that, Includes the following steps: 1) A buffer layer, a channel layer, a barrier layer, a first gate p-type GaN cap layer, an AlN insertion layer, and a second gate p-type GaN cap layer are sequentially grown on a substrate, wherein the thickness of the AlN insertion layer is 0.5~5 nm; 2) Inductively coupled plasma etching technology is used to dry etch the second gate p-type GaN cap layer using fluorine-containing etching gas. Based on the high etching selectivity between AlN and pGaN, the etching interface stops on the surface of the AlN insertion layer. Then, the sample is immersed in an alkaline solution to remove any fluorides that may be present on the AlN surface after etching. 3) Etch the AlN insertion layer and the first gate p-type GaN cap layer to form a pGaN / AlN / pGaN cap layer structure; 4) A passivation layer is grown on the barrier layer and cap layer structure; 5) Etch the passivation layer on the barrier layer to form grooves for depositing the source and drain, and then deposit the electrode metal to form the source and drain. 6) Form device isolation; 7) Etch the passivation layer on the cap layer structure to form a groove for depositing gate metal, then grow the gate metal to form the gate, and obtain a high-performance pGaN gate gallium nitride high electron mobility transistor with good device characteristic consistency.
2. The preparation method according to claim 1, characterized in that, The thickness of the first gate p-type GaN cap layer is 10~300 nm, and the thickness of the second gate p-type GaN cap layer is 2~50 nm.
3. The preparation method according to claim 1, characterized in that, The substrate is a Si substrate, a SiC substrate, a sapphire substrate, or a GaN substrate; the buffer layer is selected from one or more of the following materials: GaN, AlN, InGaN, AlGaN, and InAlGaN.
4. The preparation method according to claim 1, characterized in that, The channel layer is made of GaN, InGaN, AlGaN, or InAlGaN.
5. The preparation method according to claim 1, characterized in that, The barrier layer is selected from one or more of the following materials: GaN, AlN, AlGaN, InGaN, and InAlGaN.
6. The preparation method according to claim 1, characterized in that, The passivation layer is made of SiO2 or Si3N4.
7. The preparation method according to claim 1, characterized in that, Step 6) The method to achieve device isolation is to perform ion implantation in the passivation layer region on the side of the device to form a device isolation region. The implanted ions are selected from one or more combinations of F, N, B, Ar and Fe ions, so that the passivation layer in this region and the barrier layer and channel layer below it form a device isolation region. Alternatively, the passivation layer region on the side of the device can be etched away, removing the passivation layer and the underlying barrier and channel layers, thus eliminating the two-dimensional electron gas.
8. A pGaN gate gallium nitride high electron mobility transistor obtained by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Gallium Nitride Semiconductor Devices and Method Making Thereof
US20130112986A1
ENHANCEMENT-MODE GaN TRANSISTOR WITH SELECTIVE AND NONSELECTIVE ETCH LAYERS FOR IMPROVED UNIFORMITY IN GaN SPACER THICKNESS
US20180366559A1