Laser etching method for bioactive coating capable of sustained release of silver ions on medical titanium surface

By performing nanosecond fiber laser etching and hydrothermal reaction on the surface of medical titanium, a silver-containing titanium dioxide nanorod array coating was constructed, combined with hydroxyapatite and chitosan, to solve the bacterial infection and osseointegration of titanium alloy implants. problem, achieving precise control of the silver ion release rate and improving bone cell activity, significantly improving the biocompatibility and antibacterial ability of the implant.

CN115948733BActive Publication Date: 2024-10-11HUBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211630097.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-10-11
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

The surface of titanium and its alloy implants can easily form protective biofilms, leading to bacterial infection, and cannot form osseous combination with living bone tissue, leading to implant failure. The release rate of silver ions in existing antibacterial coatings is difficult to accurately control, and there is a lack of promotion. Bone activity.

Method used

A nanosecond fiber laser is used to perform grid etching on the surface of medical titanium to build a regular periodic structure, and a silver-containing titanium dioxide nanorod array coating is formed through hydrothermal reaction and ultrasonic cleaning, combined with hydroxyapatite and chitosan, to control Silver ion release rate and bone cell activity.

Benefits of technology

It achieves precise control of the release rate of silver ions, significantly improves the antibacterial effect and bone cell activity, enhances the biocompatibility and antibacterial ability of the implant, and ensures the safety of silver ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115948733B_ABST
    Figure CN115948733B_ABST
Patent Text Reader

Abstract

This invention discloses a laser etching method for a bioactive coating of medical titanium that can release silver ions sustainably. The method includes: first, using a fiber laser at a specific power and laser spacing to periodically process the surface of a medical titanium sheet; second, preparing a titanium dioxide nanorod array coating on the titanium sheet surface via a hydrothermal reaction, and then peeling off poorly adhered coatings by ultrasonic treatment; subsequently, loading silver nanoparticles onto the surface of the obtained array coating using a photochemical reduction method; finally, depositing a chitosan-hydroxyapatite composite coating on the aforementioned coating surface via spin coating, resulting in a highly ordered surface microarray periodic structure antibacterial composite coating. The obtained coating preparation method is simple, with high structural precision and good repeatability, which is conducive to large-scale mass production. The coating prepared by this invention has the advantages of both one-dimensional and three-dimensional structures, which can induce bone formation and achieve precise control of the silver ion release rate, thus possessing both antibacterial and bioactive properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser surface etching and material chemical preparation composite technology, and in particular to a laser etching method for a bioactive coating capable of sustained-release silver ions on the surface of medical titanium. Background Art

[0002] Titanium and its alloys have been widely used in clinical practice as repair and replacement materials for hard tissues such as artificial bones, artificial joints, and dental implants due to their excellent mechanical properties, low elastic modulus, and good biocompatibility. However, a biofilm that protects internal bacteria will form on the surface of titanium and its alloy implants, which can easily cause bacterial infection at the surgical site, resulting in surgical failure and even the death of the patient. It is reported that the postoperative bacterial infection rate in artificial joint replacement surgery is as high as 15%, which is the primary factor causing surgical failure. In addition, since the surface of titanium and its alloys is biologically inert, it cannot form bony bonds with living bone tissue and cannot induce the formation of new bone, which will eventually lead to long-term failure of the implant in the body.

[0003] In the past decade, a large number of studies on the preparation of antibacterial coatings on the surface of titanium and its alloys have been reported, especially based on TiO2 with good biocompatibility and thermal stability. 2 Silver-containing composite coatings represented by . Silver nanoparticles are a well-known broad-spectrum antibacterial material. Silver ions with a suitable release rate can not only inhibit bacteria but also promote the repair of bone tissue. However, disordered and excessive release of silver ions has a greater toxic effect on normal human cells. At present, the methods for regulating the release of silver ions in coatings mainly focus on constructing a surface barrier layer of a certain thickness on the surface of the coating to prevent nanosilver from being directly exposed to the outer surface of the coating. However, this method still has problems such as difficulty in large-scale preparation and the inability to accurately control the release rate of silver ions. Moreover, the coating structure prepared in this way generally does not have osteogenic activity and the performance is relatively simple. It is imperative to develop new silver-containing composite coatings with both excellent antibacterial and biological activity.

[0004] The construction of regular micro-nano structures and micro-nano patterns on the coating surface by laser etching technology provides an opportunity to realize this new type of coating. A femtosecond laser preparation method for the periodic structure of the antibacterial activation surface of biomedical titanium and titanium alloy (publication number CN114393312A) uses femtosecond laser technology to construct a long strip periodic structure with certain antibacterial and osteogenic activity on the surface of medical titanium, but the antibacterial and osteogenic activities of the medical titanium samples prepared by this method are not ideal. A bone-inducing medical titanium alloy with a micro-nano structure on the surface and its preparation method (publication number CN101264550A) provides a micro-nano porous structure loaded with hydroxyapatite formed on the surface of a medical titanium-calcium alloy using femtosecond laser processing, but the antibacterial effect of the alloy surface prepared by this method is poor. Silver ions play an important role in both antibacterial and osteogenic activity, but there has been no report on the method of effectively combining the sustained release regulation of silver ions with the periodic structure of the surface of medical titanium to construct a method with both excellent antibacterial and osteogenic activity. Summary of the invention

[0005] In view of the deficiencies of the prior art, the object of the present invention is to provide a laser etching method for a bioactive coating capable of sustained-release silver ions on the surface of medical titanium.

[0006] To achieve the above object, the present invention provides a method for preparing a microarray periodic structure coating on a medical titanium surface having both antibacterial and bioactive properties, comprising the following steps:

[0007] S1: After the medical titanium sheet is gradually ground and polished with sandpaper, it is ultrasonically cleaned with acetone, ethanol and deionized water respectively, and then a nanosecond fiber laser is used to perform grid etching on the surface of the medical titanium sheet at a specific power, scanning speed, frequency and laser spacing;

[0008] S2: Pre-coating the treated medical titanium sheet with a seed layer, then mixing a titanium trichloride solution and deionized water to prepare a 50 mL solution, adding sodium chloride thereto, and fully stirring the solution to obtain a hydrothermal solution, placing the titanium sheet in a hydrothermal reactor for reaction, annealing the titanium sheet after the hydrothermal reaction, ultrasonically cleaning the titanium sheet to remove a portion of the coating with poor adhesion, and then drying for standby use;

[0009] S3: immersing the obtained titanium dioxide nanorod array coating in 10 mL of silver nitrate solution of a specific concentration, irradiating it vertically with a 10 W ultraviolet lamp for a specific time, taking it out and rinsing it with deionized water, and drying it in a vacuum drying oven for 4 hours to obtain a silver-containing titanium dioxide nanorod array coating;

[0010] S4: Calcium nitrate tetrahydrate and ammonium hydrogen phosphate were fully mixed in deionized water at Ca / P=1.67 for hydrothermal reaction. The obtained product was centrifuged and annealed and calcined at 700°C for 3 hours to obtain hydroxyapatite. An appropriate amount of the obtained hydroxyapatite and 1g of chitosan were dissolved in 30 ml of acetic acid solution with a specific mass fraction. After sufficient stirring and dispersion, they were coated on the surface of the silver-containing titanium dioxide nanorod array coating obtained in S2 by spin coating, and placed in a vacuum drying oven at 37°C for 12 hours for corresponding tests.

[0011] As a preferred solution, in step S1, the power range of the nanosecond fiber laser used is 30-60W, and the scanning speed range is 2500-3500mm / s; in step S1, the frequency range of the nanosecond fiber laser used is 150-300kHz, and the laser spacing is 0.1-0.3mm.

[0012] Furthermore, in the step S2, the amount of sodium chloride added to the hydrothermal solution is in the range of 0 to 20 g, and the amount of titanium trichloride added is in the range of 0 to 2 mL; in the step S2, the reaction temperature in the hydrothermal solution is in the range of 100 to 200° C., and the reaction time is 1 to 6 hours; in the step S2, the ultrasonic cleaning conditions for removing the part of the coating with poor adhesion are 70W cleaning for 10 minutes.

[0013] Furthermore, in the step S3, the concentration range of the silver nitrate solution is 1 to 100 mM; in the step S3, the vertical irradiation time range of the ultraviolet lamp is 5 to 30 minutes.

[0014] Furthermore, in the step S4, the amount of hydroxyapatite used is in the range of 0 to 2 g; in the step S4, the mass fraction of the acetic acid solution is in the range of 1 to 5%.

[0015] Compared with the prior art, the beneficial effects and advantages of the present invention are as follows:

[0016] The present invention uses a laser etching technology that can be replicated in large quantities to prepare a series of regular periodic structures on the surface of medical titanium. By adjusting the contact area between the silver-containing coating and the water environment, the diffusion process of water molecules inside the coating is controlled, and the precise regulation of the silver ion release rate of the silver-containing composite coating is fundamentally achieved, making it more suitable for clinical medical needs. In addition, the periodic surface also has a significant inducing orientation effect on bone cells and bone tissue, and combined with the biological activity of hydroxyapatite and chitosan, it significantly promotes the proliferation and differentiation of bone cells. In particular, the present invention realizes for the first time the regulation of the release rate of silver ions in the silver-containing coating by surface structures with different grid spacings, without the need to separately prepare a surface barrier layer to control the release of silver ions; the specific advantages are as follows:

[0017] 1. The method proposed in the present invention of first preparing a grid periodic structure surface on the surface of medical titanium and its alloys by femtosecond laser etching technology, and then constructing a silver-containing composite biological coating thereon provides a new idea and method for the preparation of medical titanium implants with both antibacterial and osteogenic activity. Combined with ultrasonic treatment technology, the newly formed biological coating on the surface of medical titanium generally has good adhesion and is not easy to fall off.

[0018] 2. The grid-type periodic structure silver-loaded composite coating prepared by the present invention has an adjustable silver ion release rate. The grid spacing size is cleverly controlled by designing different laser etching parameters, and the diffusion rate of water molecules in the silver-containing coating is regulated, thereby achieving precise control of the silver ion release rate, so that it does not harm normal human cells while being antibacterial, and provides a new and simple control method for the sustained release of silver ions.

[0019] 3. The grid-shaped silver-containing composite coating prepared by the present invention has excellent antibacterial effect on Escherichia coli and Staphylococcus aureus, and the antibacterial rate of the composite coatings of all structures is higher than 85%. Compared with the antibacterial rate of medical titanium surfaces prepared by laser technology, which is generally less than 50%, the antibacterial rate is significantly improved (publication number CN 114393312A, publication number CN101264550A).

[0020] 4. The gridded silver-containing composite coating structure prepared by the present invention is very conducive to the adhesion and growth of osteoblasts. After one week of co-culture, the activity of osteoblasts in the coating without the addition of hydroxyapatite-chitosan is greater than 90%, while the activity of osteoblasts in the coating after the addition of hydroxyapatite-chitosan can reach up to more than 110%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 These are metallographic microscope images of the surface of medical titanium sheets with laser spacing of (a) 0.1 mm, (b) 0.15 mm, and (c) 0.2 mm;

[0022] Figure 2 This is the SEM image of the surface of a titanium sheet coated with a 10% Ag-loaded titanium dioxide nanorod array with a laser spacing of 0.1 mm;

[0023] in: Figure 2 (a) SEM scale bar is 20 μm; Figure 2 (b) SEM scale is 100 μm (including side view).

[0024] Figure 3 It is an ICP-MS test curve of silver ion release of titanium dioxide nanorod array coating with 10% Ag content without laser etching and when the laser etching intervals are 0.1mm, 0.15mm and 0.2mm respectively;

[0025] Figure 4This is the SEM image of the composite coating with 10% Ag content with a laser spacing of 0.15 mm;

[0026] in: Figure 4 (a) Figure 4 (b) is the SEM image of the composite coating with 10% Ag content without hydroxyapatite when the laser spacing is 0.15 mm; Figure 4 (c) Figure 4 (d) is the SEM image of the composite coating with 10% Ag content when the laser spacing is 0.15 mm and the hydroxyapatite content is 0.5 g; Figure 4 (e) Figure 4 (f) is the SEM image of the composite coating with 10% Ag content and a laser spacing of 0.15 mm and a hydroxyapatite content of 1.5 g.

[0027] Figure 5 These are the fluorescence images obtained using an inverted fluorescence microscope after the 10% Ag content titanium dioxide nanorod array coating was co-cultured in MC3T3-E1 cells for 48 hours and then stained when the laser etching spacing was (a) 0.1 mm, (b) 0.15 mm, and (c) 0.2 mm. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.

[0029] Example 1: Laser Etching Preparation of Silver-Containing Periodic Structure Coating without Hydroxyapatite-Chitosan

[0030] S1: A nanosecond fiber laser was used to perform array etching on the surface of a medical titanium sheet at a power of 40 W, a scanning speed of 2700 mm / s, and a frequency of 180 kHz. The laser spacing was set to 0.1 mm, 0.15 mm, and 0.2 mm (e.g. Figure 1 shown).

[0031] S2: The treated medical titanium sheet is pre-coated with a seed layer, and then 1.75 mL of titanium trichloride solution and deionized water are mixed to prepare a 50 mL solution, 12 g of sodium chloride is added thereto, and the solution is fully stirred to obtain a hydrothermal solution, and the titanium sheet is placed in a hydrothermal reactor for a reaction at 190 degrees Celsius for 6 hours. After the hydrothermal reaction is completed, the titanium sheet is annealed to obtain a titanium dioxide nanorod array coating;

[0032] S3: The obtained titanium dioxide nanorod array coating was immersed in 10 mL of 10 mM silver nitrate solution (10% Ag content), irradiated vertically with a 10 W ultraviolet lamp for 20 minutes, rinsed with deionized water, and dried in a vacuum drying oven for 4 hours to obtain a silver-containing titanium dioxide nanorod array coating (the sample SEM with a laser spacing of 0.15 mm is as follows Figure 2 As shown). The obtained coating was subjected to ICP-MS silver ion release rate test, and it can be observed that the laser etching spacing has a significant regulatory and sustained release effect on the silver ion release of the coating. Within 7 days, the silver ion release rate of the sample without surface etching was the largest (180μg / L), the release rate of the sample with a laser spacing of 0.2mm was 130μg / L, the release rate of the sample with a laser spacing of 0.15mm was 115μg / L, and the release rate of the sample with a laser spacing of 0.1mm was 100μg / L, with a precise sustained release regulation gradient, indicating that the laser etching spacing has a significant effect on the precise regulation of the silver ion release rate. All samples have excellent antibacterial effects on Escherichia coli and Staphylococcus aureus, with an antibacterial rate of more than 90%, and the antibacterial effect is better with the increase of the silver ion release rate.

[0033] Example 2: Laser etching preparation of silver-containing periodic structure coating with hydroxyapatite-chitosan

[0034] S1: A nanosecond fiber laser was used to perform array etching on the surface of a medical titanium sheet at a power of 40 W, a scanning speed of 2700 mm / s, and a frequency of 180 kHz. The laser spacing was set to 0.15 mm, 0.15 mm, and 0.2 mm (e.g. Figure 1 shown).

[0035] S2: The treated medical titanium sheet is pre-coated with a seed layer, and then 1.75 mL of titanium trichloride solution and deionized water are mixed to prepare a 50 mL solution, 12 g of sodium chloride is added thereto, and the solution is fully stirred to obtain a hydrothermal solution, and the titanium sheet is placed in a hydrothermal reactor for a reaction at 190 degrees Celsius for 6 hours. After the hydrothermal reaction is completed, the titanium sheet is annealed to obtain a titanium dioxide nanorod array coating;

[0036] S3: The obtained titanium dioxide nanorod array coating was immersed in 10 mL of 10 mM silver nitrate solution (10% Ag content), irradiated vertically with a 10 W ultraviolet lamp for 20 minutes, rinsed with deionized water, and dried in a vacuum drying oven for 4 hours to obtain a silver-containing titanium dioxide nanorod array coating (the sample SEM with a laser spacing of 0.15 mm is as follows Figure 2 shown);

[0037] S4: Calcium nitrate tetrahydrate and ammonium hydrogen phosphate were fully mixed in deionized water at a Ca / P ratio of 1.67 for hydrothermal reaction. The obtained product was centrifuged and annealed at 700°C for 3 hours to obtain hydroxyapatite. 0g, 0.5g and 1.5g of hydroxyapatite and 1g of chitosan were respectively dissolved in 30 ml of 2% acetic acid solution by mass fraction. After being fully stirred and dispersed, they were coated on the surface of the silver-containing titanium dioxide nanorod array coating obtained in S3 by spin coating, and placed in a vacuum drying oven at 37°C for 12 hours. The obtained samples were as shown in Figure 4 As shown. The silver ion release rate test shows that the higher the hydroxyapatite content, the lower the silver ion release rate, which reduces the antibacterial effect of the sample, but it is still greater than 85%. The osteoblast activity test shows that for the same sample, by setting different laser spacing, the cell adhesion and growth state will also have significant differences. Figure 5 The results showed that cells had the best adhesion and spreading performance when the laser spacing was 0.15 mm, while reducing (0.1 mm) or increasing (0.2 mm) the spacing would inhibit the adhesion and growth of osteoblasts to a certain extent.

Claims

1. A laser etching method for a bioactive coating capable of sustained-release of silver ions on a medical titanium surface, characterized in that: The following steps are included: S1: After the medical titanium sheet was gradually ground and polished with sandpaper, it was ultrasonically cleaned with acetone, ethanol and deionized water respectively, and then the surface of the medical titanium sheet was grid-etched with a nanosecond fiber laser at a specific power, scanning speed, frequency and laser spacing; the power range of the nanosecond fiber laser used was 30 ~ 60 W, and the scanning speed range was 2500 ~ 3500 mm / s; the frequency range of the nanosecond fiber laser used was 150 ~ 300 kHz, and the laser spacing was 0.1 ~ 0.3 mm; S2: Pre-coat the treated medical titanium sheet with a seed layer, then mix the titanium trichloride solution and deionized water to prepare a 50 mL solution, add sodium chloride thereto, stir the solution thoroughly to obtain a hydrothermal solution, and place the titanium sheet in a hydrothermal reactor for reaction; after the hydrothermal reaction is completed, the titanium sheet is annealed, ultrasonically cleaned to remove the coating with poor adhesion, and then dried for standby use; S3: Immerse the obtained titanium dioxide nanorod array coating in a 10 mL silver nitrate solution of a specific concentration, irradiate it vertically with a 10 W ultraviolet lamp for a specific time, take it out and rinse it with deionized water, and dry it in a vacuum drying oven for 4 hours to obtain a silver-containing titanium dioxide nanorod array coating; the concentration range of the silver nitrate solution is 1 to 100 mM; the vertical irradiation time range of the ultraviolet lamp is 5 to 30 minutes; S4: Calcium nitrate tetrahydrate and ammonium hydrogen phosphate are fully mixed in deionized water at a Ca / P ratio of 1.67 for hydrothermal reaction. The obtained product is centrifuged and annealed and calcined at 700°C for 3 hours to obtain hydroxyapatite; an appropriate amount of the obtained hydroxyapatite and 1 g of chitosan are dissolved in 30 ml of acetic acid solution with a specific mass fraction, and after sufficient stirring and dispersion, they are coated on the surface of the silver-containing titanium dioxide nanorod array coating obtained in step S2 by spin coating, and placed in a vacuum drying oven at 37°C for 12 hours, and corresponding tests are performed; the amount of hydroxyapatite used ranges from 0 to 2 g; the mass fraction of the acetic acid solution ranges from 1 to 5%.

2. The laser etching method for the bioactive coating capable of sustained-release of silver ions on the surface of medical titanium according to claim 1, characterized in that: In step S2, the amount of sodium chloride added to the hydrothermal solution is in the range of 0 to 20 g, and the amount of titanium trichloride added is in the range of 0 to 2 mL; In step S2, the reaction temperature in the hydrothermal solution ranges from 100 to 200° C., and the reaction time ranges from 1 to 6 hours; In step S2, the ultrasonic cleaning condition for removing the portion of the coating with poor adhesion is 70 W for 10 min.