A composite adsorption material for rare earth recovery and preparation method thereof

By functionalizing methyl methacrylate and modified soil graphite, unearthed graphite composite PMMA carboxylated adsorption microspheres are prepared, which solves the problems of complexity and low efficiency of rare earth adsorption materials, and achieves high efficiency and no Poisonous, low-cost rare earth recycling effect.

CN115970660BActive Publication Date: 2024-11-15HUBEI INST OF GEOLOGICAL SCI (HUBEI INST OF SELENIUM RICH IND)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310026662.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-15
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The existing rare earth adsorption materials have problems such as complex application processes, fragility, easy to poison and low adsorption efficiency, making it difficult to achieve low-cost, high adsorption capacity and non-toxic rare earth recovery.

Method used

The functional transformation of methyl methacrylate (PMMA) and modified soil graphite is used for functional transformation. Through the synergistic action of inorganic substances and polymer phases, unearthed graphite composite PMMA carboxylated adsorption microspheres are prepared, which improves the adsorption capacity of rare earths. And reduces the preparation cost and toxicity of the material.

Benefits of technology

It significantly improves the adsorption capacity of rare earths, the material is non-toxic and not fragile, and the application method is simple. It overcomes the shortcomings of traditional adsorbent materials, has a high specific surface area and pore structure, and is suitable for efficient recycling of rare earth elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115970660B_ABST
    Figure CN115970660B_ABST
Patent Text Reader

Abstract

The present invention provides a composite adsorption material for rare earth recovery and a preparation method thereof, and relates to the technical field of rare earth resource recovery and utilization. The present invention uses methyl methacrylate (PMMA) as a monomer, mixes it with modified earthy graphite for functionalization transformation, and prepares a composite adsorption material for rare earth recovery under certain conditions. The present invention utilizes the synergistic effect between inorganic matter and polymer phase, overcomes the common problems of existing rare earth adsorption materials, significantly improves the rare earth adsorption capacity of the adsorption material, and the adsorption material has the advantages of low preparation cost, non-toxicity and non-fragility. The composite adsorption material of the present invention is used to adsorb rare earths in rare earth beneficiation waste liquid, and can effectively recover rare earth resources in the waste liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rare earth resource recovery and utilization, and in particular to a composite adsorption material for rare earth recovery and a preparation method thereof. Background Art

[0002] Rare earth elements are a general term for 17 elements in the periodic table, including lanthanide elements (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), and yttrium (Y) and scandium (Sc), which are closely related to the 15 elements of the lanthanide series. Rare earth elements have very special electronic structures and excellent physical and chemical properties. They are widely used in important fields such as the national defense industry and the electronics industry. They can produce fluorescent materials, rare earth metal hydride battery materials, electric light source materials, permanent magnet materials, hydrogen storage materials, catalytic materials, precision ceramic materials, laser materials, superconducting materials, magnetostrictive materials, magnetocold materials, magneto-optical storage materials, optical fiber materials, etc. They are important raw materials necessary for the development of high-tech industries.

[0003] With the rapid development of science and technology, a large amount of rare earth metals have entered the environment, which has not only had an adverse impact on the environment and human health, but also led to a large amount of waste of rare earth metals. Therefore, the recycling of rare earth resources is not only conducive to the utilization of rare earth resources, but also has a positive impact on environmental protection. At present, the recovery of rare earth elements generally requires the help of adsorption materials. However, existing rare earth adsorption materials, such as ion exchange resins, generally have problems such as poor waste liquid treatment effect. The main reasons are as follows: ① The application process of adsorption materials is not yet popular and the application method is relatively complicated. In actual application, it is difficult to correctly set the application conditions and process parameters according to the specific situation; ② The defects in the performance of the adsorption material itself, such as fragility, easy poisoning, low adsorption efficiency, etc.; ③ The application method of the adsorption material is single.

[0004] Therefore, how to provide a composite adsorption material for rare earth recovery with low cost, high adsorption capacity, non-toxicity, non-fragility and simple application method and its preparation method is one of the technical problems that need to be solved urgently. Summary of the invention

[0005] In order to solve the above problems, the present invention uses methyl methacrylate (PMMA) as a monomer, mixes it with modified earthy graphite for functionalization, and prepares a composite adsorption material for rare earth recovery under certain conditions, namely earthy graphite composite PMMA carboxylation adsorption microspheres. The present invention utilizes the synergistic effect between inorganic matter and polymer phase, overcomes the common problems of existing rare earth adsorption materials, significantly improves the rare earth adsorption capacity of the adsorption material, and the adsorption material has the advantages of low preparation cost, non-toxicity and non-fragile.

[0006] The method for preparing the composite adsorption material for rare earth recovery of the present invention comprises the following steps:

[0007] (1) mixing a dispersant polyvinyl alcohol solution and deionized water, heating the mixture to 42° C., and stirring the mixture to obtain a mixture A;

[0008] (2) mixing the initiator with the monomer and the cross-linking agent, adding modified earthy graphite after the solid is dissolved, and ultrasonically dispersing for 15 minutes to obtain a mixture B;

[0009] (3) mixing the porogen and kerosene evenly, pouring the mixture into mixture B, and stirring evenly to obtain mixture C;

[0010] (4) Mixture C was quickly poured into mixture A, and the reaction system was heated to 75°C for 1 h, then heated to 85°C for 1 h, and finally heated to 90°C for aging for 0.5 h.

[0011] (5) After the reaction is completed, stop heating and stirring, wash the solid product three times with hot water, and dry it at 40°C to constant weight;

[0012] (6) using petroleum ether to Soxhlet extract the solid product in a water bath at 70° C. for 8 h. After the extraction, the product was dried at room temperature to obtain earthy graphite composite PMMA microspheres;

[0013] (7) After soaking the soil-like graphite composite PMMA microspheres with furfuryl alcohol for 10 hours, the system was heated to 80°C and a hot NaOH solution was added. After stirring evenly, the system was heated to 130°C and refluxed for 3 hours to remove water and furfuryl alcohol. After the reaction was completed, the system was cooled to 90°C, rinsed with deionized water for 3 times, filtered and dried, and extracted with anhydrous ethanol for 8 hours. After the product was taken out and dried, the finished composite adsorbent material for rare earth recovery was obtained.

[0014] Furthermore, in the step (1), the concentration of the polyvinyl alcohol solution is 1%-8%.

[0015] Furthermore, in the step (1), the weight ratio of polyvinyl alcohol to deionized water is 1-8:100.

[0016] Furthermore, in step (2), the initiator is benzoyl peroxide, the monomer is methyl methacrylate, and the crosslinking agent is divinylbenzene.

[0017] Furthermore, the modified earthy graphite in step (2) is one or more of γ-methacryloxypropyltrimethoxysilane modified earthy graphite, sodium dodecyl sulfate modified earthy graphite and sodium hexadecylbenzene sulfonate modified earthy graphite.

[0018] Furthermore, the preparation method of the γ-methacryloxypropyltrimethoxysilane modified earthy graphite is as follows: weigh 10.0 g of earthy graphite and place it in a 250 mL three-necked flask, add 100 mL of 3 mol / L H2SO4 solution thereto, heat to 90° C. and react for 12 h, after the reaction is completed, rinse with deionized water 3 times, filter, place in an oven at 80° C. and dry, and bag for later use, to obtain acidified earthy graphite;

[0019] Weigh 2.0 g of the acidified earthy graphite prepared in the above experiment and place it in a 250 mL three-necked flask, pour 50 mL of toluene solution into it, stir evenly, continue to add 10 mL of γ-methacryloxypropyltrimethoxysilane into the three-necked flask, heat to 75 ° C and react for 6 hours. After the reaction is completed, rinse with solvent 3 times, filter, place in an oven at 80 ° C for constant temperature drying, and bag for later use, which is γ-methacryloxypropyltrimethoxysilane modified earthy graphite.

[0020] Furthermore, the preparation method of the sodium dodecyl sulfate modified earthy graphite is as follows: weigh 2.0g of sodium dodecyl sulfate and place it in a 250mL three-necked flask, pour 50mL of deionized water into it, stir until the solid is completely dissolved, add 2.0g of the acidified earthy graphite prepared in the above experiment into the above three-necked flask, stir evenly, heat to 85°C and react for 6h, after the reaction is completed, rinse with deionized water 3 times, filter, place in an oven at 80°C for constant temperature drying, and bag for later use, which is the sodium dodecyl sulfate modified earthy graphite.

[0021] Furthermore, the preparation method of the sodium hexadecylbenzene sulfonate modified earthy graphite is as follows: weigh 2.0g of sodium hexadecylbenzene sulfonate and place it in a 250mL three-necked flask, pour 50mL of deionized water into it, stir until the solid is completely dissolved, add 2.0g of the acidified earthy graphite prepared in the above experiment into the above three-necked flask, stir evenly, heat to 80°C and react for 6h, after the reaction is completed, rinse with deionized water 3 times, filter, place in an oven at 80°C for constant temperature drying, and bag for later use, which is the sodium hexadecylbenzene sulfonate modified earthy graphite.

[0022] Furthermore, in the step (2), the weight ratio of the monomer, the cross-linking agent and the modified earthy graphite is 1:0.03-0.07:0.005-0.025.

[0023] Furthermore, the porogen in step (3) is toluene, and the volume ratio of the porogen to kerosene is 2-6:5-9.

[0024] Furthermore, in step (7), the concentration of the NaOH hot solution is 20wt%-60wt%, and the temperature of the NaOH hot solution is 50-70°C.

[0025] Preferably, the concentration of the NaOH hot solution in step (7) is 30wt%-50wt%.

[0026] Furthermore, in the step (7), the weight ratio of the earthy graphite composite PMMA microspheres to the NaOH hot solution is 1:1.

[0027] Another object of the present invention is to protect a composite adsorption material for rare earth recovery prepared according to the above method.

[0028] Earthy graphite has good acid and alkali resistance, and participates in polymer polymerization as a second phase, effectively improving the performance defects of PMMA and reducing the cost of material synthesis. The present invention uses earthy graphite composite PMMA microspheres as a substrate, performs functional transformation in a furfuryl alcohol system, introduces -COOH into the composite microsphere structure, and utilizes the synergistic effect between inorganic matter and polymer phase to improve the adsorption capacity of earthy graphite composite PMMA carboxyl adsorption microspheres, and enables them to maintain more pores during preparation and use, thereby having a higher specific surface area, which is more conducive to the adsorption of rare earth ions and increases the adsorption capacity.

[0029] The present invention utilizes the ion exchange principle to achieve efficient adsorption of rare earth elements. The —COONa on the structural skeleton of the composite adsorption material of the present invention can dissociate into Na + , Na + The rare earth ions in the solution diffuse from the solution into the composite adsorbent material structure to achieve adsorption of rare earth elements. The exchange driving force of the composite adsorbent material of the present invention is the concentration difference between the two ions. The greater the concentration difference, the greater the absorption of rare earth ions and Na + The faster the exchange rate, when this exchange reaction reaches a certain extent, the exchange between the two reaches a dynamic equilibrium state.

[0030] In the actual application process, the composite adsorbent material of the present invention is placed in a solution containing a strong electrolyte. The rare earth ion diffusion caused by the obvious concentration difference between the solid phase and the solution phase of the adsorbent material disturbs the electrical neutrality and causes a potential difference between the earthy graphite composite PMMA carboxylated adsorbent microspheres and the solution phase. This potential difference is the Donnan potential. The Donnan potential tends to pull the ions with opposite charges into the corresponding phase, thereby obtaining an ion diffusion tendency caused by the concentration difference. When it reaches a state of equilibrium with the phase where the potential field exists, the adsorption of the rare earth ions is completed.

[0031] Compared with the prior art, the beneficial technical effects of the present invention are:

[0032] The present invention overcomes the shortcomings of traditional rare earth adsorption materials, utilizes the synergistic effect between inorganic matter and polymer phase, functionalizes the adsorption material, significantly improves the rare earth adsorption capacity of the adsorption material, and the adsorption material has the advantages of low preparation cost, non-toxicity and non-fragility. At the same time, the earthy graphite of the present invention can be dispersed in the sample after functionalization, proving that the functionalization of the material of the present invention has no adverse effect on the addition of the second phase, ensuring the performance of the material in subsequent applications. The composite adsorption material for rare earth recovery of the present invention is used for rare earth adsorption in rare earth beneficiation waste liquid, which has important practical significance for the conservation and recovery of important strategic resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention will be further described below in conjunction with the accompanying drawings.

[0034] Figure 1 SEM images of the composite adsorption material for rare earth recovery prepared in Example 1 of the present invention (a×1000; b, c, d×3000; e, f×5000; g, h×10000). DETAILED DESCRIPTION

[0035] The technical solution provided by the present invention is further described below in conjunction with embodiments.

[0036] Example 1

[0037] A method for preparing a composite adsorption material for rare earth recovery, comprising the following steps:

[0038] 1. Add 20g of deionized water to a clean 250mL three-necked flask, weigh 1.0g of polyvinyl alcohol and add it to the reaction flask, heat to 42℃ and stir until the two are evenly mixed;

[0039] 2. Weigh 0.1 g of initiator benzoyl peroxide and place it in a dry 100 mL conical flask, add 10.0 g of methyl methacrylate monomer and 0.45 g of crosslinker divinylbenzene, and after the solid is dissolved, add 0.15 g of sodium hexadecylbenzenesulfonate modified earthy graphite to the conical flask and disperse it in an ultrasonic disperser for 15 min;

[0040] 3. Add 6 mL of porogen toluene and 15 mL of kerosene to a dry 100 mL beaker, mix well and pour into the above-mentioned evenly dispersed conical flask;

[0041] 4. Quickly pour the mixture in the conical flask into the above three-necked flask, start stirring, heat to 75℃ for reaction for 1h, then heat to 85℃ for reaction for 1h, then heat to 90℃ for aging for 0.5h;

[0042] 5. After the reaction is completed, stop heating and stirring, pour out the liquid in the three-necked flask, wash the solid product three times with hot water, and dry it in a constant temperature drying oven at 40°C to constant weight;

[0043] 6. Pour 100 mL of petroleum ether into a dry 250 mL round-bottom flask, place the above product in a Soxhlet extractor, connect it to the round-bottom flask, place it in a constant temperature water bath at 70 ° C for 48 hours, and after the extraction, pour the product into a watch glass and dry it at room temperature to obtain earthy graphite composite PMMA microspheres;

[0044] 7. Weigh 10.0g of dry earthy graphite composite PMMA microspheres and place them in a 250mL three-necked flask, add 8mL of furfuryl alcohol and soak for 10h, heat to 80℃, add 10.0g of 60℃ 50wt% NaOH solution, stir evenly, heat to 130℃ and reflux for 3h, remove water and methanol with a water separator, after the reaction is completed, cool to 90℃, rinse with deionized water 3 times, filter and dry, place the dried crude product in a Soxhlet extractor, extract with ethanol for 8h, take out and dry to obtain a composite adsorption material for rare earth recovery.

[0045] The adsorption capacity of the prepared composite adsorbent material for rare earth recovery was measured, and the results were as follows: Eu(III) 182.20 mg / g, Dy(III) 192.60 mg / g, Tb(III) 210.36 mg / g.

[0046] Example 2

[0047] 1. Add 20g of deionized water to a clean 250mL three-necked flask, weigh 0.4g of polyvinyl alcohol and add it to the reaction flask, heat to 42℃ and stir until the two are evenly mixed;

[0048] 2. Weigh 0.1 g of initiator benzoyl peroxide and place it in a dry 100 mL conical flask, add 10.0 g of methyl methacrylate monomer and 0.60 g of crosslinker divinylbenzene, and after the solid is dissolved, add 0.20 g of γ-methacryloxypropyltrimethoxysilane modified earthy graphite to the conical flask and disperse it in an ultrasonic disperser for 15 min;

[0049] 3. Add 4 mL of porogen toluene and 6 mL of kerosene to a dry 100 mL beaker, mix well and pour into the above-mentioned evenly dispersed conical flask;

[0050] 4. Quickly pour the mixture in the conical flask into the above three-necked flask, start stirring, heat to 75℃ for reaction for 1h, then heat to 85℃ for reaction for 1h, then heat to 90℃ for aging for 0.5h;

[0051] 5. After the reaction is completed, stop heating and stirring, pour out the liquid in the three-necked flask, wash the solid product three times with hot water, and dry it in a constant temperature drying oven at 40°C to constant weight;

[0052] 6. Pour 100 mL of petroleum ether into a dry 250 mL round-bottom flask, place the above product in a Soxhlet extractor, connect it to the round-bottom flask, place it in a constant temperature water bath at 70 ° C for 48 hours, and after the extraction, pour the product into a watch glass and dry it at room temperature to obtain earthy graphite composite PMMA microspheres;

[0053] 7. Weigh 10.0g of dry earthy graphite composite PMMA microspheres and place them in a 250mL three-necked flask, add 6mL of furfuryl alcohol and soak for 10h, heat to 80℃, add 10.0g of 50℃ 30% NaOH solution, stir evenly, heat to 130℃ and reflux for 3h, remove water and methanol with a water separator, after the reaction is completed, cool to 90℃, rinse with deionized water 3 times, filter and dry, place the dried crude product in a Soxhlet extractor, extract with ethanol for 8h, take out and dry to obtain a composite adsorption material for rare earth recovery.

[0054] The adsorption capacity of the prepared composite adsorbent material for rare earth recovery was measured, and the results were as follows: Eu(III) 178.62 mg / g, Dy(III) 184.74 mg / g, Tb(III) 190.95 mg / g.

[0055] Example 3

[0056] 1. Add 20g of deionized water to a clean 250mL three-necked flask, weigh 1.6g of polyvinyl alcohol and add it to the reaction flask, heat to 42℃ and stir until the two are evenly mixed;

[0057] 2. Weigh 0.1g of initiator benzoyl peroxide and place it in a dry 100mL conical flask, add 10.0g of methyl methacrylate monomer and 0.40g of cross-linking agent divinylbenzene, and after the solid is dissolved, add 0.25g of soil-like graphite modified by sodium dodecyl sulfate to the conical flask and disperse it in an ultrasonic disperser for 15 minutes;

[0058] 3. Add 3 mL of porogen toluene and 6 mL of kerosene to a dry 100 mL beaker, mix well and pour into the above evenly dispersed conical flask;

[0059] 4. Quickly pour the mixture in the conical flask into the above three-necked flask, start stirring, heat to 75℃ for reaction for 1h, then heat to 85℃ for reaction for 1h, then heat to 90℃ for aging for 0.5h;

[0060] 5. After the reaction is completed, stop heating and stirring, pour out the liquid in the three-necked flask, wash the solid product three times with hot water, and dry it in a constant temperature drying oven at 40°C to constant weight;

[0061] 6. Pour 100 mL of petroleum ether into a dry 250 mL round-bottom flask, place the above product in a Soxhlet extractor, connect it to the round-bottom flask, place it in a constant temperature water bath at 70 ° C for 48 hours, and after the extraction, pour the product into a watch glass and dry it at room temperature to obtain earthy graphite composite PMMA microspheres;

[0062] 7. Weigh 10.0g of dry earthy graphite composite PMMA microspheres and place them in a 250mL three-necked flask, add 9mL of furfuryl alcohol and soak for 10h, heat to 80℃, add 10.0g of 80℃ 40% NaOH solution, stir evenly, heat to 130℃ and reflux for 3h, remove water and methanol with a water separator, and after the reaction is completed, cool to 90℃, rinse with deionized water 3 times, filter and dry, place the dried crude product in a Soxhlet extractor, extract with ethanol for 8h, take out and dry to obtain a composite adsorption material for rare earth recovery.

[0063] The adsorption capacity of the prepared composite adsorbent material for rare earth recovery was measured, and the results were as follows: Eu(III) 175.04 mg / g, Dy(III) 190.00 mg / g, Tb(III) 206.41 mg / g.

[0064] Test Example 1

[0065] The composite adsorbent material for rare earth recovery prepared in Example 1 of the present invention was used as an example, and the commercially available D113 weak acid ion exchange resin was used as a comparative example. The saturated adsorption capacity, saturated adsorption capacity, and adsorption reduction ratio after repeated use for 6 times were tested. The results are as follows:

[0066]

[0067] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing a composite adsorbent material for rare earth recovery, characterized in that: The following steps are involved: (1) Mixing a dispersant polyvinyl alcohol and deionized water, heating the mixture to 42° C., and stirring the mixture to obtain a mixture A; (2) Mixing the initiator with the monomer and the cross-linking agent, adding the modified earthy graphite after the solid is dissolved, and ultrasonically dispersing for 15 minutes to obtain a mixture B; (3) Mix the porogen and kerosene evenly, pour into mixture B, and stir evenly to obtain mixture C; (4) Mixture C was quickly poured into mixture A. The reaction system was heated to 75°C for 1 h, then heated to 85°C for 1 h, and finally heated to 90°C for aging for 0.5 h. (5) After the reaction is completed, stop heating and stirring, wash the solid product three times with hot water, and dry it at 40°C to constant weight; (6) The solid product was subjected to Soxhlet extraction with petroleum ether in a water bath at 70°C for 8 h. After the extraction, the product was dried at room temperature to obtain earthy graphite composite PMMA microspheres. (7) After soaking the soil-like graphite composite PMMA microspheres with furfuryl alcohol for 10 h, the system was heated to 80 °C and a hot NaOH solution was added. After stirring evenly, the system was heated to 130 °C and refluxed for 3 h to remove water and furfuryl alcohol. After the reaction was completed, the system was cooled to 90 °C, rinsed with deionized water for 3 times, filtered and dried, and extracted with anhydrous ethanol for 8 h. After the product was taken out and dried, the finished composite adsorbent material for rare earth recovery was obtained; The modifier for modifying the earthy graphite in step (2) is one or more of γ-methacryloxypropyltrimethoxysilane, sodium dodecyl sulfate and sodium hexadecylbenzenesulfonate; In the step (2), the weight ratio of the monomer, the cross-linking agent and the modified earthy graphite is 1:0.04:0.025; In step (7), the concentration of the NaOH hot solution is 20wt%-60wt%, and the temperature of the NaOH hot solution is 50-70°C; In the step (7), the weight ratio of the earthy graphite composite PMMA microspheres to the NaOH hot solution is 1:1; The rare earth elements are Eu(III), Dy(III) and Tb(III).

2. The method for preparing a composite adsorbent material for rare earth recovery according to claim 1, characterized in that: In the step (1), the weight ratio of polyvinyl alcohol to deionized water is 1-8:

100.

3. The method for preparing a composite adsorbent material for rare earth recovery according to claim 1, characterized in that: In step (2), the initiator is benzoyl peroxide, the monomer is methyl methacrylate, and the crosslinking agent is divinylbenzene.

4. The method for preparing a composite adsorbent material for rare earth recovery according to claim 1, characterized in that: The porogen in step (3) is toluene, and the volume ratio of the porogen to kerosene is 2-6:5-9.

5. A composite adsorbent material for rare earth recovery, characterized in that: Prepared by the method according to any one of claims 1 to 4.