A method for preparing graphene-modified polyamide 6 filaments
By grafting halamine monomer on the surface of graphene oxide and adding antibacterial agents and combining fillers, graphene modified polyamide 6 filaments are prepared, which solves the problems of dispersion and antibacterial properties of graphene in aqueous solution, and achieves more lasting antibacterial effect and better spinning properties.
Patent Information
- Application Number
- CN202211717825.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-29
AI Technical Summary
In the prior art, graphene is difficult to disperse evenly in aqueous solution, resulting in limited antibacterial properties and insufficient antibacterial effect.
Graphene modified polyamide 6 filaments are prepared by grafting halamine monomers on the surface of graphene oxide, adding fillers, guanidine antibacterial agents and quaternary ammonium antibacterial agents, and ring-opening polymerization with lactam to improve its dispersion and antibacterial properties.
It enhances the dispersion and antibacterial properties of graphene, extends the antibacterial time, improves the antibacterial ability of polyamide 6 composite fiber, and improves the mechanical strength and spinability of the fiber.
Smart Images

Figure BDA0004026963220000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamides, and in particular to a method for preparing graphene-modified polyamide 6 filaments. Background Art
[0002] Polyamide 6 fiber is a polycaprolactam fiber obtained by ring-opening polymerization of caprolactam monomer and then spinning. It is currently widely used in spinning and engineering plastics. In recent years, the antibacterial properties of composite materials have received widespread attention. Graphene belongs to carbon materials and is a kind of sp 2 Graphene is a two-dimensional material composed of hybrid C atoms, which has good elasticity and excellent fracture strength. Therefore, the use of graphene is becoming more and more extensive. Graphene has a large specific surface area and is widely used in biomedicine. In addition, graphene oxide, an oxidized derivative of graphene, has broad-spectrum antibacterial properties. When it comes into contact with bacteria, it causes irreversible damage to the bacterial cell membrane and is biocompatible. Some studies have used graphene oxide and monomer caprolactam to obtain polyamide 6 composite fibers. The addition of graphene oxide has improved the antibacterial properties of polyamide 6 composite fibers to a certain extent. However, as people's requirements for environmental hygiene are increasing, how to obtain polyamide 6 composite fibers with higher antibacterial ability has become a research focus.
[0003] The patent with application number CN2021107184006 introduces a method for preparing a graphene disinfectant, which includes adding a dispersant to graphene and obtaining a homogeneous and stable dispersion by ultrasonic treatment. Then, a non-ionic surfactant and a quaternary ammonium salt are added to the stable graphene dispersion for mixed reaction to obtain a graphene disinfectant. Although the bactericidal effect is improved by the synergistic effect of graphene and quaternary ammonium salt, it is difficult to disperse the graphene evenly because salts easily cause graphene to agglomerate. Summary of the invention
[0004] In order to improve the uniformity of graphene dispersion, improve its antibacterial performance, and further prepare graphene-modified polyamide 6 filaments, the present invention provides a method for preparing graphene-modified polyamide 6 filaments.
[0005] A method for preparing graphene-modified polyamide 6 filaments comprises the following steps:
[0006] S1: Grafting halamine monomers onto the surface of graphene oxide under the action of a catalyst to obtain halamine-modified graphene;
[0007] S2: adding fillers, guanidine antibacterial agents and quaternary ammonium salt antibacterial agents to the halamine-modified graphene to react and obtain antibacterial modified graphene;
[0008] S3: Dispersing the antibacterial modified graphene in deionized water, adding caprolactam, and obtaining a polymerized fluid after ring opening and polymerization, and then slicing, extracting, drying, and spinning to obtain graphene-modified polyamide filaments.
[0009] Furthermore, the preparation method is specifically as follows:
[0010] S1: dissolving graphene oxide in deionized water, adding halamine monomer, ultrasonically mixing, adding potassium persulfate as a catalyst, heating to 60-70°C, reacting for 3-5h, washing, drying, and extracting to obtain halamine-modified graphene;
[0011] S2: dissolving the halamine-modified graphene in deionized water, adding filler, guanidine antibacterial agent and quaternary ammonium salt antibacterial agent, ultrasonically dispersing, adding 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, reacting at 30-40° C. for 24-26 hours, washing and drying to obtain the antibacterial modified graphene;
[0012] S3: Dispersing the antibacterial modified graphene in deionized water, adding caprolactam, and obtaining a polymerized fluid after ring opening and polymerization, and then slicing, extracting, drying, and spinning to obtain graphene-modified polyamide filaments.
[0013] Furthermore, the preparation method of the halamine monomer is as follows: sodium hydroxide and 5,5-dimethylhydantoin are dissolved in deionized water, 3-chloro-1-propanol is added, the mixture is reacted at 100-110° C. for 10-12 hours, and the mixture is distilled under reduced pressure. After acetone is added, the mixture is filtered and distilled under reduced pressure, and the mixture is evenly mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride is added in an ice bath. After the mixture is reacted for 1-2 hours, the mixture is reacted at room temperature for 20-24 hours, and the mixture is purified and distilled under reduced pressure to obtain the halamine monomer.
[0014] Furthermore, the preparation method of the quaternary ammonium salt antibacterial agent is as follows: dissolving dodecaned tertiary amine in a dichloromethane solution, adding benzyl bromide, reacting at 40-50° C., adding anhydrous ether, filtering and drying to obtain the quaternary ammonium salt antibacterial agent.
[0015] Furthermore, the preparation method of the guanidine antibacterial agent is as follows: nitrogen is introduced, N,N-dimethylacetamide and o-toluene biguanide hydrochloride are mixed, dodecylamine is added, the temperature is raised to 130-160° C., the reaction is carried out for 24-26 hours, and the guanidine antibacterial agent is separated and purified.
[0016] Furthermore, the filler is one or more of titanium dioxide, zinc oxide, zirconium dioxide, and vanadium trioxide.
[0017] Furthermore, the preparation of the antibacterial modified graphene includes the following raw materials in parts by weight: 0.4-1 part of graphene oxide, 4-10 parts of halamine monomers, 4-8 parts of fillers, 8-12 parts of guanidine antibacterial agents and 8-12 parts of quaternary ammonium salt antibacterial agents.
[0018] Furthermore, the mass ratio of the dodecaned tertiary amine to the benzyl bromide is 1:(0.8-1.2).
[0019] Furthermore, the mass dosage ratio of the o-toluidine hydrochloride to the dodecylamine is 1:(1-1.5).
[0020] Compared with the prior art, this application has the following beneficial effects:
[0021] 1. The halamine monomer is used to react with the hydroxyl groups on the surface of graphene oxide, and the halamine monomer is grafted on the surface of graphene oxide to reduce the surface roughness, improve the dispersibility of graphene oxide, expose more sharp edges of graphene oxide, increase the contact area between graphene oxide and bacteria, and spin the modified graphene and caprolactam to obtain a polyamide 6 composite fiber with better antibacterial properties. In addition, graphene oxide is used as a carrier of the halamine monomer, so that the halamine monomer has good storage stability and sustained release effect, and the antibacterial effect of graphene oxide is stable and the antibacterial time is extended, and the antibacterial ability of the obtained polyamide 6 composite fiber is more durable. At the same time, the two are combined through covalent bonds, which improves the thermal stability of the oxygen-containing groups on the surface of graphene oxide.
[0022] 2. Guanidine antimicrobial agents and quaternary ammonium salt antimicrobial agents are both organic antimicrobial agents. Adding these two antimicrobial agents to graphene oxide can greatly improve the antimicrobial properties of graphene. In addition, the introduction of benzyl groups into quaternary ammonium salt antimicrobial agents can improve the inhibitory effect on fungi and bacteria. The antimicrobial properties of guanidine antimicrobial agents can be further improved by extending the carbon chain. However, guanidine antimicrobial agents are salts, which make graphene oxide easy to agglomerate. By grafting halamine monomers on the surface of graphene oxide, the agglomeration of graphene oxide in aqueous solution is inhibited.
[0023] 3. Fillers are added to graphene. The fillers will be loaded between the graphene oxide sheets, reducing the van der Waals force and the π-π force between the sheets, and improving the dispersibility of the graphene oxide. The loading of the fillers will play a supporting role between the sheets, which can improve the mechanical strength and hardness of the graphene oxide. In addition, the fillers are all photocatalytic substances, which use high-temperature reactions to kill most of the bacteria, further improving the antibacterial properties of graphene, so that the polyamide 6 composite fiber obtained from the modified graphene and caprolactam has stronger antibacterial properties and better spinnability. DETAILED DESCRIPTION
[0024] The present application is further described below in conjunction with specific embodiments.
[0025] In Examples 1-4 of the present application, the graphene oxide is selected from Changzhou Sixth Element Materials Technology Co., Ltd., model SE2430W-N; in Example 5 of the present application, homemade graphene oxide is selected.
[0026] Example 1
[0027] A graphene-modified polyamide 6 filament is prepared by the following method:
[0028] Step 1: Dissolve 20 parts of dodecylamine in 80 parts of dichloromethane solution, heat to 40°C, add 20 parts of benzyl bromide, react for 24 hours, add anhydrous ether, precipitate the product, and dry to obtain a quaternary ammonium salt antibacterial agent;
[0029] Step 2: Pass nitrogen, mix 20 parts of N,N-dimethylacetamide and 1 part of o-toluene biguanide hydrochloride evenly, slowly drop 1 part of dodecylamine, heat to 130°C, react for 24 hours, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0030] Step 3: dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 100 parts of deionized water, add 20 parts of 3-chloro-1-propanol, heat to 100°C, react for 10 hours, distill under reduced pressure, add 20 parts of acetone, filter, distill under reduced pressure, mix evenly with 10 parts of tetrahydrofuran, add 20 parts of triethylamine, add 30 parts of acryloyl chloride in an ice bath, react for 1 hour, react at room temperature for 20 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0031] Step 4: Dissolve 0.5 parts of graphene oxide in 100 parts of deionized water, add 5 parts of halamine monomer, ultrasonically react for 0.5 hours, mix evenly with 0.2 parts of potassium persulfate, heat to 60 ° C, react for 3 hours, centrifuge, wash, dry, grind, extract for 48 hours, dry, mix evenly with 50 parts of water, add 5 parts of titanium dioxide, 10 parts of guanidine antibacterial agent and 10 parts of quaternary ammonium antibacterial agent, ultrasonically react for 15 minutes, add 5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 10 minutes, cool to 30 ° C, react for 24 hours, centrifuge, wash and dry to obtain modified graphene.
[0032] Step 5: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of modified graphene to caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then carry out a ring-opening reaction at 270°C for 2.5h, and then polymerize at 250°C for 6.5h to obtain a polymerized fluid, and then pass the fluid into a pelletizer for slicing, and then place the slices in an extraction tower, extract with 90°C deionized water, and dry the extracted slices in a drying tank with nitrogen, and melt spinning to obtain modified polyamide 6 filaments. The spinning process is specifically as follows: screw temperature 265-270°C, spinning box temperature 275°C, spinning pressure 160bar, side sleeping wind cooling, measured blowing temperature 50°C, humidity 70%, wind speed 0.18m / s, oiling amount 2%, spinning winding speed 4000r / min.
[0033] Example 2
[0034] A graphene-modified polyamide 6 filament is prepared by the following method:
[0035] Step 1: Dissolve 20 parts of dodecylamine in 85 parts of dichloromethane solution, heat to 43°C, add 16 parts of benzyl bromide, react for 24.5 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0036] Step 2: Pass nitrogen, mix 20 parts of N,N-dimethylacetamide and 1 part of o-toluene biguanide hydrochloride, slowly drop 1.2 parts of dodecylamine, heat to 135°C, react for 24.5h, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0037] Step 3: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 105 parts of deionized water, add 23 parts of 3-chloro-1-propanol, heat to 105°C, react for 10.5 hours, distill under reduced pressure, add 21 parts of acetone, filter, distill under reduced pressure, mix evenly with 11 parts of tetrahydrofuran, add 20 parts of triethylamine, add 31 parts of acryloyl chloride in an ice bath, react for 1.1 hours, react at room temperature for 21 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0038] Step 4: Dissolve 0.7 parts of graphene oxide in 105 parts of deionized water, add 6 parts of halamine monomer, ultrasonically react for 0.6 hours, mix evenly with 0.3 parts of potassium persulfate, heat to 62 ° C, react for 4 hours, centrifuge, wash, dry, grind, extract for 48.5 hours, dry, mix evenly with 55 parts of water, add 3.5 parts of titanium dioxide and 3.5 parts of zirconium dioxide, 8 parts of guanidine antibacterial agents and 8 parts of quaternary ammonium antibacterial agents, ultrasonically react for 16 minutes, add 5.5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 11 minutes, cool to 36 ° C, react for 25 hours, centrifuge, wash, and dry to obtain modified graphene.
[0039] Step 5: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0040] Example 3
[0041] A graphene-modified polyamide 6 filament is prepared by the following method:
[0042] Step 1: Dissolve 20 parts of dodecylamine in 90 parts of dichloromethane solution, heat to 45°C, add 24 parts of benzyl bromide, react for 25 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0043] Step 2: Pass nitrogen, mix 25 parts of N,N-dimethylacetamide and 2 parts of o-toluene biguanide hydrochloride, slowly drop 3 parts of dodecylamine, heat to 140°C, react for 26 hours, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0044] Step 3: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 110 parts of deionized water, add 20 parts of 3-chloro-1-propanol, heat to 108°C, react for 11 hours, distill under reduced pressure, add 22 parts of acetone, filter, distill under reduced pressure, mix evenly with 12 parts of tetrahydrofuran, add 15 parts of triethylamine, add 32 parts of acryloyl chloride in an ice bath, react for 1.2 hours, react at room temperature for 21 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0045] Step 4: Dissolve 1 part of graphene oxide in 110 parts of deionized water, add 10 parts of halamine monomer, ultrasonically react for 0.7 hours, mix evenly with 0.4 parts of potassium persulfate, heat to 67 ° C, react for 3.5 hours, centrifuge, wash, dry, grind, extract for 49 hours, dry, mix evenly with 60 parts of water, add 8 parts of zirconium dioxide, 9 parts of guanidine antibacterial agent and 9 parts of quaternary ammonium antibacterial agent, ultrasonically react for 17 minutes, add 6 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 12 minutes, cool to 32 ° C, react for 25 hours, centrifuge, wash and dry to obtain modified graphene.
[0046] Step 5: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0047] Example 4
[0048] A graphene-modified polyamide 6 filament is prepared by the following method:
[0049] Step 1: Dissolve 20 parts of dodecylamine in 100 parts of dichloromethane solution, heat to 47°C, add 18 parts of benzyl bromide, react for 25.5 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0050] Step 2: Pass nitrogen, mix 25 parts of N,N-dimethylacetamide and 3 parts of o-toluene biguanide hydrochloride, slowly drop 4 parts of dodecylamine, heat to 150°C, react for 25.5h, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0051] Step 3: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 115 parts of deionized water, add 18 parts of 3-chloro-1-propanol, heat to 103°C, react for 11.5 hours, distill under reduced pressure, add 23 parts of acetone, filter, distill under reduced pressure, mix evenly with 13 parts of tetrahydrofuran, add 24 parts of triethylamine, add 33 parts of acryloyl chloride in an ice bath, react for 2 hours, react at room temperature for 22 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0052] Step 4: Dissolve 0.8 parts of graphene oxide in 115 deionized water, add 9 parts of halamine monomer, ultrasonically react for 0.8 hours, mix evenly with 0.5 parts of potassium persulfate, heat to 65°C, react for 5 hours, centrifuge, wash, dry, grind, extract for 49.5 hours, dry, mix evenly with 65 parts of water, add 6 parts of vanadium trioxide, 12 parts of guanidine antibacterial agent and 11 parts of quaternary ammonium antibacterial agent, ultrasonically react for 19 minutes, add 6.5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 14 minutes, cool to 34°C, react for 26 hours, centrifuge, wash and dry to obtain modified graphene.
[0053] Step 5: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0054] Example 5
[0055] A graphene-modified polyamide 6 filament is prepared by the following method:
[0056] Step 1: Cool down to 5°C, add 10 parts of sodium nitrate and 9 parts of graphite to 120 parts of concentrated sulfuric acid, react for 1 hour, heat to 20°C, add 20 parts of potassium permanganate in 3 batches, react for 1-1.5 hours, continue to heat to 40°C, react for 2 hours, add 200 parts of deionized water, quickly heat to 100°C, mix evenly with 16 parts of 30% hydrogen peroxide, filter, wash and dry to obtain graphene oxide;
[0057] Step 2: Dissolve 20 parts of dodecanamine in 110 parts of dichloromethane solution, heat to 50°C, add 24 parts of benzyl bromide, react for 26 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0058] Step 3: Pass nitrogen, mix 30 parts of N,N-dimethylacetamide and 5 parts of o-toluene biguanide hydrochloride, slowly drop 5 parts of dodecylamine, heat to 160°C, react for 26 hours, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0059] Step 4: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 120 parts of deionized water, add 22 parts of 3-chloro-1-propanol, heat to 110°C, react for 12 hours, distill under reduced pressure, add 24 parts of acetone, filter, distill under reduced pressure, mix evenly with 10 parts of tetrahydrofuran, add 19 parts of triethylamine, add 34 parts of acryloyl chloride in an ice bath, react for 1.5 hours, react at room temperature for 24 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0060] Step 5: Dissolve 0.4 parts of graphene oxide in 120 parts of deionized water, add 4 parts of halamine monomer, ultrasonically react for 1 hour, mix evenly with 0.6 parts of potassium persulfate, heat to 70 ° C, react for 4.5 hours, centrifuge, wash, dry, grind, extract for 50 hours, dry, mix evenly with 70 parts of water, add 4 parts of zinc oxide, 8 parts of guanidine antibacterial agent and 10 parts of quaternary ammonium antibacterial agent, ultrasonically react for 20 minutes, add 7 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 20 minutes, cool to 40 ° C, react for 24.5 hours, centrifuge, wash, and dry to obtain modified graphene. The spinning process is the same as in Example 1.
[0061] Step 6: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5h, and then polymerize at 250°C for 6.5h to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0062] Comparative Example 1
[0063] A modified polyamide 6 filament is prepared by the following method:
[0064] Step 1: Dissolve 20 parts of dodecylamine in 80 parts of dichloromethane solution, heat to 40°C, add 20 parts of benzyl bromide, react for 24 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0065] Step 2: Pass nitrogen, mix 20 parts of N,N-dimethylacetamide and 1 part of o-toluene biguanide hydrochloride, slowly drop 1 part of dodecylamine, heat to 130°C, react for 24 hours, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0066] Step 3: Mix 0.5 parts of graphene oxide with 100 parts of water, add 5 parts of titanium dioxide, 10 parts of guanidine antibacterial agent and 10 parts of quaternary ammonium antibacterial agent, ultrasonically react for 15 minutes, add 5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 10 minutes, cool to 30°C, react for 24 hours, centrifuge, wash and dry to obtain modified graphene.
[0067] Step 4: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0068] Comparative Example 2
[0069] A modified polyamide 6 filament is prepared by the following method:
[0070] Step 1: Dissolve 20 parts of dodecylamine in 80 parts of dichloromethane solution, heat to 40°C, add 20 parts of benzyl bromide, react for 24 hours, add anhydrous ether, precipitate the product, and dry it to obtain a quaternary ammonium salt antibacterial agent;
[0071] Step 2: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 100 parts of deionized water, add 20 parts of 3-chloro-1-propanol, heat to 100°C, react for 10 hours, distill under reduced pressure, add 20 parts of acetone, filter, distill under reduced pressure, mix evenly with 10 parts of tetrahydrofuran, add 20 parts of triethylamine, add 30 parts of acryloyl chloride in an ice bath, react for 1 hour, react at room temperature for 20 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0072] Step 3: Dissolve 0.5 parts of graphene oxide in 100 parts of deionized water, add 5 parts of halamine monomer, ultrasonically react for 0.5 hours, mix evenly with 0.2 parts of potassium persulfate, heat to 60 ° C, react for 3 hours, centrifuge, wash, dry, grind, extract for 48 hours, dry, mix evenly with 50 parts of water, add 5 parts of titanium dioxide and 20 parts of quaternary ammonium antibacterial agent, ultrasonically react for 15 minutes, add 5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 10 minutes, cool to 30 ° C, react for 24 hours, centrifuge, wash and dry to obtain modified graphene.
[0073] Step 4: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0074] Comparative Example 3
[0075] A modified polyamide 6 filament is prepared by the following method:
[0076] Step 1: Pass nitrogen, mix 20 parts of N,N-dimethylacetamide and 1 part of o-toluene biguanide hydrochloride evenly, slowly drop 1 part of dodecylamine, heat to 130°C, react for 24 hours, evaporate the solvent, separate and purify to obtain a guanidine antibacterial agent;
[0077] Step 2: Dissolve 20 parts of sodium hydroxide and 20 parts of 5,5-dimethylhydantoin in 100 parts of deionized water, add 20 parts of 3-chloro-1-propanol, heat to 100°C, react for 10 hours, distill under reduced pressure, add 20 parts of acetone, filter, distill under reduced pressure, mix evenly with 10 parts of tetrahydrofuran, add 20 parts of triethylamine, add 30 parts of acryloyl chloride in an ice bath, react for 1 hour, react at room temperature for 20 hours, purify, and distill under reduced pressure to obtain a halamine monomer;
[0078] Step 3: Dissolve 0.5 parts of graphene oxide in 100 parts of deionized water, add 5 parts of halamine monomer, ultrasonically react for 0.5 hours, mix evenly with 0.2 parts of potassium persulfate, heat to 60 ° C, react for 3 hours, centrifuge, wash, dry, grind, extract for 48 hours, dry, mix evenly with 50 parts of water, add 5 parts of titanium dioxide and 20 parts of guanidine antibacterial agent, ultrasonically react for 15 minutes, add 5 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, continue ultrasonic reaction for 10 minutes, cool to 30 ° C, react for 24 hours, centrifuge, wash and dry to obtain modified graphene.
[0079] Step 4: Disperse the modified graphene in deionized water, add liquid caprolactam, wherein the mass ratio of the modified graphene to the caprolactam is 1:100, obtain a mixed solution by ultrasound and high-speed shearing, then perform a ring-opening reaction at 270°C for 2.5 hours, and then polymerize at 250°C for 6.5 hours to obtain a polymerized fluid, then pass the fluid into a pelletizer to slice, then place the slices in an extraction tower, extract with 90°C deionized water, dry the extracted slices in a drying tank with nitrogen, and melt-spin to obtain modified polyamide 6 filaments. The spinning process is the same as in Example 1.
[0080] The spinning properties of different modified polyamide 6 filaments were compared, and the antibacterial rate of modified polyamide 6 filaments was tested. Escherichia coli and Staphylococcus aureus were used as test bacteria. The test steps were based on GB / T20944.3-2008. First, the concentration of live bacteria in the flask at "0" contact time was tested, recorded as W0, and then the number of colonies was tested at oscillation contact times of 18h, 1 month, and 3 months, recorded as W. t The results are shown in Table 1. The calculation formula of the antibacterial rate Y is as follows: Y = (W t -W0) / W0×100%.
[0081] Table 1 Test results of filaments of Examples 1-5 and Comparative Examples 1-3
[0082]
[0083] From the antibacterial rate data of the modified polyamide 6 filaments, it can be seen that the antibacterial rate of comparative example 1 is significantly lower than that of examples 1-5, and the antibacterial rate in examples 1-5 is still maintained at a high level at 1 month and 3 months, while the durability of the antibacterial rate of the modified polyamide 6 filaments obtained in comparative example 1 is poor, which further illustrates that the modification of the halamine monomer can keep the antibacterial rate of the modified polyamide 6 stable. It can be seen from the spinning performance test that when the halamine monomer is added, the appearance of the modified polyamide 6 filaments is free of lint, the molding is good, the full roll rate effect is good, and it has better spinnability.
[0084] Compared with Examples 1-5, the antibacterial properties of Comparative Examples 2 and 3 are both reduced. When modifying graphene, adding a quaternary ammonium antibacterial agent alone without adding a guanidine antibacterial agent, or adding a guanidine antibacterial agent alone without adding a quaternary ammonium antibacterial agent, both reduce the antibacterial property of the modified graphene, indicating that the compound of quaternary ammonium antibacterial agents and guanidine antibacterial agents can improve the antibacterial property of graphene.
[0085] The above specific implementation methods are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A method for preparing graphene-modified polyamide 6 filaments, characterized in that: The following steps are involved: S1: Grafting halamine monomers onto the surface of graphene oxide under the action of a catalyst to obtain halamine-modified graphene; S2: adding fillers, guanidine antibacterial agents, quaternary ammonium salt antibacterial agents and 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride to the halamine-modified graphene to react and obtain antibacterial modified graphene; S3: dispersing the antibacterial modified graphene in deionized water, adding caprolactam, ring-opening and polymerizing to obtain a polymerized fluid, and then slicing, extracting, drying, and spinning to obtain graphene-modified polyamide filaments; The preparation method of the halamine monomer is as follows: sodium hydroxide and 5,5-dimethylhydantoin are dissolved in deionized water, 3-chloro-1-propanol is added, the mixture is reacted at 100-110° C. for 10-12 hours, and vacuum distillation is performed. After acetone is added, the mixture is filtered and vacuum distilled, and the mixture is evenly mixed with tetrahydrofuran, triethylamine is added, acryloyl chloride is added in an ice bath, the mixture is reacted for 1-2 hours, the mixture is reacted at room temperature for 20-24 hours, and the mixture is purified and vacuum distilled to obtain the halamine monomer. The filler is one or more of titanium dioxide, zinc oxide, zirconium dioxide and vanadium trioxide.
2. The method for preparing graphene-modified polyamide 6 filament according to claim 1, characterized in that: The preparation method is specifically: S1: dissolving graphene oxide in deionized water, adding halamine monomer, ultrasonically mixing, adding potassium persulfate as a catalyst, heating to 60-70°C, reacting for 3-5h, washing, drying, and extracting to obtain halamine-modified graphene; S2: dissolving the halamine-modified graphene in deionized water, adding filler, guanidine antibacterial agent and quaternary ammonium salt antibacterial agent, ultrasonically dispersing, adding 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, reacting at 30-40° C. for 24-26 hours, washing and drying to obtain the antibacterial modified graphene; S3: Dispersing the antibacterial modified graphene in deionized water, adding caprolactam, and obtaining a polymerized fluid after ring opening and polymerization, and then slicing, extracting, drying, and spinning to obtain graphene-modified polyamide filaments.
3. The method for preparing graphene-modified polyamide 6 filament according to claim 1, characterized in that: The preparation method of the quaternary ammonium salt antibacterial agent is as follows: dissolving dodecaned tertiary amine in a dichloromethane solution, adding benzyl bromide, reacting at 40-50° C., adding anhydrous ether, filtering and drying to obtain the quaternary ammonium salt antibacterial agent.
4. The method for preparing graphene-modified polyamide 6 filament according to claim 1, characterized in that: The preparation method of the guanidine antibacterial agent is as follows: nitrogen is introduced, N,N-dimethylacetamide and o-toluene biguanide hydrochloride are mixed, dodecylamine is added, the temperature is raised to 130-160° C., the reaction is carried out for 24-26 hours, and the guanidine antibacterial agent is separated and purified.
5. The method for preparing graphene-modified polyamide 6 filament according to claim 3, characterized in that: The mass ratio of the dodecaned tertiary amine to the benzyl bromide is 1:(0.8-1.2).
6. The method for preparing graphene-modified polyamide 6 filament according to claim 4, characterized in that: The mass dosage ratio of the o-toluidine hydrochloride to the dodecylamine is 1:(1-1.5).