Liquid Ammonia Pretreatment Technology of Regenerated Cellulose Fiber Fabric
Patent Information
- Application Number
- CN202211687608.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-27
Smart Images

Figure BDA0004020067730000111 
Figure HDA0004020067740000011 
Figure HDA0004020067740000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textiles, and in particular relates to a liquid ammonia pretreatment process for regenerated cellulose fiber fabrics. Background Art
[0002] Regenerated cellulose fiber has the characteristics of wide range of raw materials, recyclable and reusable, and natural degradation, which meets the needs of today's society for eco-friendly environment. At the same time, regenerated cellulose fiber has the characteristics of soft touch, soft luster, moisture absorption and breathability, anti-static, good drape, and performance similar to silk, and is gradually becoming a new fashion trend. However, the dimensional stability, wrinkle resistance and wear resistance of fabrics containing regenerated cellulose fibers are poor. After liquid ammonia finishing, the regenerated cellulose fabrics have improved dimensional stability, good resilience, fabric flatness, texture clarity, fullness and smoothness.
[0003] Regenerated cellulose fibers mainly include Tencel, cuprammonium, viscose, modal, bamboo fiber, etc. Taking viscose fiber as an example, it is made of natural fiber (wood fiber, cotton linter) as raw material, and is made into soluble cellulose xanthate through alkalization, aging, sulfonation and other processes, and then dissolved in dilute alkali solution to make spinning solution. After filtering, maturation and degassing, the solution is wet-spun, and the viscose is chemically reacted with a coagulation bath composed of sulfuric acid, sodium sulfate and zinc sulfate. The sodium cellulose xanthate in the viscose reacts with the sulfuric acid in the coagulation bath and decomposes to obtain cellulose fiber, which is made into finished products through washing, desulfurization, bleaching, oiling, drying and other procedures. The purpose of oiling is to reduce the friction coefficient of the fiber, reduce electrostatic reaction, make the fiber soft and smooth, and improve the spinnability of the fiber. The oil agent is mainly quaternary ammonium salt and fatty acid. At present, some new types of regenerated cellulose fiber oil agents are added in a variety of ways, and many manufacturers do not disclose them as core secrets, which brings many difficulties to dyeing and finishing.
[0004] In practice, we have found that when the content of regenerated cellulose in the fabric is high, for example, when the content of regenerated cellulose fiber reaches more than 60%, the probability of shiny oil marks appearing in the fabric during liquid ammonia finishing will greatly increase. The probability of occurrence of different types of fibers is also different. For example, the probability of oil marks appearing in Tencel and Lyocell is relatively high, which brings great uncertainty to the liquid ammonia finishing of such fabrics. If liquid ammonia is not processed, many properties of the fiber cannot be improved. Therefore, solving the problem of contamination at the oil outlet points of liquid ammonia in the processing of regenerated cellulose fibers has become the key to improving the performance of such fiber fabrics. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a liquid ammonia pretreatment process for regenerated cellulose fiber fabrics, so as to solve the problem of contamination of such fabrics at the oil outlet points caused by liquid ammonia during dyeing and finishing, reduce the defective rate and rework rate, reduce production costs, and improve the wearing performance of such fabrics.
[0006] The liquid ammonia pretreatment process of the regenerated cellulose fiber fabric of the present invention comprises the following steps:
[0007] Singeing → cold stacking → oxygen bleaching → stentering → liquid ammonia.
[0008] in:
[0009] The cold stacking process is to roll and stack the steel sheets after dipping into the working liquid.
[0010] The working solution formula is: degreasing agent TF-109H: 4-8 g / L, long-chain fatty alcohol polyoxyethylene ether refining agent: 4-8 g / L, caustic soda: 30-50 g / L, desizing enzyme: 4-8 g / L, penetrant: 4-6 g / L. Among them, the long-chain fatty alcohol polyoxyethylene ether refining agent is preferably SA-U produced by Zibo Lurui Fine Chemical Co., Ltd.; the desizing enzyme is preferably DS-HT produced by Zibo Lurui Fine Chemical Co., Ltd.; the penetrant is preferably WA-M produced by Zibo Lurui Fine Chemical Co., Ltd.
[0011] The coiling and stacking temperature is 38-42° C. and the time is 10-12 hours.
[0012] In the oxygen bleaching process, degreasing agent TF-109H: 4-8 g / L, caustic soda: 3-5 g / L, hydrogen peroxide: 18-22 g / L, hydrogen peroxide stabilizer: 6-8 g / L, chelating agent: 8-12 g / L, penetrant: 4-6 g / L, steam oven temperature 101°C for 25 min. Among them, the hydrogen peroxide stabilizer is preferably OUR-266 produced by Nantong Aoer Industry and Trade Co., Ltd., the chelating agent is preferably SQ-N produced by Zibo Lurui Fine Chemical Co., Ltd.; the penetrant is preferably WA-M produced by Zibo Lurui Fine Chemical Co., Ltd.
[0013] In the study, it was found that through high-power microscope observation, the regenerated cellulose fibers (viscose and modal, respectively) at the oil print after liquid ammonia finishing showed obvious signs of damage, such as Figure 1 , Figure 2 shown.
[0014] In order to further prevent oil leakage caused by fiber damage, the present invention adds a liquid ammonia pre-stretching finishing step, and adds a fiber protective agent during the stretching finishing, which can effectively prevent the damage of the regenerated cellulose fiber. The specific implementation process is as follows:
[0015] The stentering process is performed by dipping the fiber protective agent of fatty acid amide in working solution, and the drying temperature is 120-150° C. and the drying time is 30 seconds. The fatty acid amide fiber protective agent is preferably PARASOFTENER CS produced by Qingdao Dayuan Chemical Co., Ltd.
[0016] The working solution concentration of the fatty acid amide fiber protective agent is 20-30 g / L.
[0017] The liquid ammonia processing procedure adopts the process of "fast exchange and high liquid supply", that is, lowering the liquid level of the ammonia tank from the original 70% to 30-40%, and controlling the increase of the liquid amount of the fabric from the original 55-65% to 75-80%. In this way, on the one hand, the accumulation of oil in the ammonia tank can be reduced by increasing the exchange speed of ammonia liquid in the ammonia tank, and at the same time, the increase in liquid amount can also effectively ensure the effect of liquid ammonia finishing, and make up for the reduction of liquid ammonia finishing effect caused by insufficient immersion time at low liquid level.
[0018] The specific implementation process is: ammonia tank liquid level 30-40%, rolling rate 75-80%, vehicle speed 50-60m / min, treatment chamber temperature 60-70℃, steam chamber temperature 110-120℃, water washing tank temperature 50-60℃, overflow water 400-600L / h.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention redesigns the pretreatment and liquid ammonia processing process of the regenerated cellulose fiber fabric. The conventional processing process is: singeing → deboiling → oxygen bleaching → liquid ammonia, and the newly designed dyeing and finishing process is: singeing → cold stacking → oxygen bleaching → stentering → liquid ammonia.
[0021] (2) The present invention adopts a cold stacking process with low energy consumption. A high-efficiency degreasing agent and a refining agent are added during the cold stacking process to form a synergistic effect. Compared with the single use of a refining agent, the effect is better. In addition, the high-efficiency degreasing agent has a wide adaptability and can effectively remove the spinning oil on a variety of regenerated cellulose fibers.
[0022] (3) The present invention adds a degreasing agent during the oxygen bleaching process. During the oxygen bleaching process, hydrogen peroxide has a certain destructive effect on the fiber. At the same time, the oil in the fiber will be further dissolved under high temperature conditions, thereby improving the oil dissolution efficiency.
[0023] (4) The present invention effectively reduces the spinning oil in the regenerated cellulose fiber. The regenerated cellulose fiber fabric is treated by this process flow, which can effectively avoid the oil spot contamination problem caused by the dissolution of the spinning oil during liquid ammonia finishing.
[0024] (5) The process of the present invention has wide adaptability and is applicable to common regenerated cellulose fibers such as viscose, tencel, cuprammonium, modal, bamboo fiber, etc.
[0025] (6) The fabrics treated by the process of the present invention can effectively improve their quality when processed to be soft or non-ironing finish. The regenerated cellulose fiber fabrics processed with liquid ammonia have stable fabric dimensions, good resilience, smooth fabric surface, clear texture, and are plump and smooth. The tear strength of the regenerated cellulose fiber fabrics processed with liquid ammonia is increased by about 10%, and the non-ironing property is increased by about 0.3 level. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the viscose fiber at the oil print after liquid ammonia finishing, magnified 1000 times.
[0027] Figure 2 This is a 1000-fold magnified SEM image of the Modal fiber at the oil print site after liquid ammonia finishing. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto.
[0029] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0030] Degreasing agent TF-109H was purchased from Zhejiang Chuanhua Group Co., Ltd.;
[0031] Desizing enzyme DS-HT, penetrant WA-M, refining agent SA-U, and chelating agent SQ-N were purchased from Zibo Lurui Fine Chemical Co., Ltd.;
[0032] Hydrogen peroxide stabilizer OUR-266 was purchased from Nantong Aoer Industry and Trade Co., Ltd.;
[0033] The fiber protective agent PARASOFTENER CS was purchased from Qingdao Dayuan Chemical Co., Ltd.
[0034] Example 1
[0035] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0036] The liquid ammonia pretreatment process for the regenerated cellulose fiber fabric of the present invention comprises the following steps: singeing→cold stacking→oxygen bleaching→stentering→liquid ammonia.
[0037] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0038] Cold stacking: degreasing agent TF-109H: 4g / L, refining agent SA-U: 4g / L, desizing enzyme DS-HT: 4g / L, penetrant WA-M: 4g / L, caustic soda 30g / L, stacking temperature 38℃, stacking time 10h.
[0039] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 4g / L, caustic soda (45Be): 3g / L, hydrogen peroxide (27.5%): 18g / L, chelating agent SQ-N: 8g / L, hydrogen peroxide stabilizer OUR-266: 6g / L, penetrant WA-M: 4g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0040] Stretching: fiber protection agent PARASOFTENER CS: 20g / L, drying temperature 120℃, drying time 30s, using Monforts stenter.
[0041] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 30%, rolling rate 75%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0042] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0043] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0044] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0045] Using the process of Example 1, the finished cloth surface has no oil spot stains.
[0046] Example 2
[0047] Specifications: CM50*TENCEL40*150*90*57 / 58, structure: 1 / 1+31 / 11, pure cotton in warp direction + 100% Tencel in weft direction, weight: 120±10g / m 2 .
[0048] The liquid ammonia pretreatment process for the regenerated cellulose fiber fabric of the present invention comprises the following steps: singeing→cold stacking→oxygen bleaching→stentering→liquid ammonia.
[0049] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0050] Cold stacking: degreasing agent TF-109H: 6g / L, refining agent SA-U: 6g / L, desizing enzyme DS-HT: 6g / L, penetrant WA-M: 5g / L, caustic soda 40g / L, stacking temperature 40℃, stacking time 12h.
[0051] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 6g / L, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 5g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0052] Stretching: fiber protection agent PARASOFTENER CS: 25g / L, drying temperature 130℃, drying time 30s, using Monforts stenter.
[0053] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 35%, rolling rate 78%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0054] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0055] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0056] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0057] Using the process of Example 2, the finished cloth surface has no oil spot stains.
[0058] Example 3
[0059] Specifications: TENCEL CPT60*C / BEM CPT50*240*120*57 / 58, structure: 4 / 1 satin, composition: 26.2% cotton, 62.5% Tencel, 11.3% cuprammonium, weight 150±10g / m 2 .
[0060] The liquid ammonia pretreatment process for the regenerated cellulose fiber fabric of the present invention comprises the following steps: singeing→cold stacking→oxygen bleaching→stentering→liquid ammonia.
[0061] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0062] Cold stacking: degreasing agent TF-109H: 8g / L, refining agent SA-U: 8g / L, desizing enzyme DS-HT: 8g / L, penetrant WA-M: 6g / L, caustic soda 50g / L, stacking temperature 42℃, stacking time 12h.
[0063] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 8g / L, caustic soda (45Be): 5g / L, hydrogen peroxide (27.5%): 22g / L, chelating agent SQ-N: 12g / L, hydrogen peroxide stabilizer OUR-266: 8g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0064] Stretching: fiber protection agent PARASOFTENER CS: 30g / L, drying temperature 150℃, drying time 30s, using Monforts stenter.
[0065] Liquid ammonia: vehicle speed 60m / min, ammonia tank liquid level 40%, rolling rate 78%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0066] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0067] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0068] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0069] Using the process of Example 3, the finished cloth surface has no oil spot stains.
[0070] Comparative Example 1
[0071] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0072] Conventional process: singeing → deboiling → oxygen bleaching → liquid ammonia.
[0073] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0074] Deboiling: caustic soda: 40g / L, desizing enzyme DS-HT: 3g / L, penetrant WA-M: 4g / L, refining agent SA-U: 4g / L, chelating agent SQ-N: 5g / L, vehicle speed: 80m / min, steamer temperature: 98℃, piling time: 15min, PVA washing zone temperature (℃): no heating, 85, 85, 85, 85, training water washing zone temperature (℃): 95, 95, 95, 80, overflow water: 4L / kg, using Beninger deboiling machine.
[0075] Oxygen bleaching: vehicle speed: 70m / min, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0076] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 70%, rolling rate 58%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0077] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0078] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0079] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0080] Using the process of Comparative Example 1, the oil spot stain score of the finished cloth was 374 points / 100 yards.
[0081] Comparative Example 2
[0082] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0083] Cold stacking without degreasing agent process: singeing → cold stacking → oxygen bleaching → stretching → liquid ammonia.
[0084] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0085] Cold stacking: desizing enzyme DS-HT: 6g / L, refining agent SA-U: 4g / L, penetrant WA-M: 4g / L, caustic soda 40g / L, stacking temperature 40℃, stacking time 12h.
[0086] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 8g / L, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0087] Stretching: fiber protection agent PARASOFTENER CS: 20g / L, drying temperature 150℃, drying time 30s, using Monforts stenter.
[0088] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 40%, rolling rate 75%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0089] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0090] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0091] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0092] Using the process of Comparative Example 2, the oil spot stain score of the finished cloth was 53 points / 100 yards.
[0093] Comparative Example 3
[0094] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0095] Oxygen bleaching without degreasing agent process: singeing → cold stacking → oxygen bleaching → stenting → liquid ammonia.
[0096] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0097] Cold stacking: degreasing agent TF-109H: 8g / L, refining agent SA-U: 4g / L, desizing enzyme DS-HT: 6g / L, penetrant WA-M: 4g / L, caustic soda 40g / L, stacking temperature 40℃, stacking time 12h.
[0098] Oxygen bleaching: vehicle speed: 70m / min, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0099] Stretching: fiber protection agent PARASOFTENER CS: 20g / L, drying temperature 150℃, drying time 30s, using Monforts stenter.
[0100] Liquid ammonia: speed 50m / min, ammonia tank level 40%, rolling rate 75%, treatment room temperature 65℃, steam chamber temperature 120℃, washing tank temperature 50℃, overflow water 600L / h. Use Japan Kyoto liquid ammonia finishing machine.
[0101] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0102] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0103] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0104] Using the process of Comparative Example 3, the oil spot stain score of the finished cloth was 18 points / 100 yards.
[0105] Comparative Example 4
[0106] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0107] Stretching process without adding fiber protective agent: singeing → cold stacking → oxygen bleaching → stretching → liquid ammonia.
[0108] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0109] Cold stacking: degreasing agent TF-109H: 8g / L, refining agent SA-U: 4g / L, desizing enzyme DS-HT: 6g / L, penetrant WA-M: 4g / L, caustic soda 40g / L, stacking temperature 40℃, stacking time 12h.
[0110] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 8g / L, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0111] Stretching: water squeezing, drying temperature 150℃, drying time 30s, using Monforts stenter.
[0112] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 40%, rolling rate 75%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0113] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0114] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0115] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0116] Using the process of Comparative Example 4, the oil spot stain score of the finished cloth was 31 points / 100 yards.
[0117] Comparative Example 5
[0118] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m2 .
[0119] Conventional process of liquid ammonia: singeing → cold stacking → oxygen bleaching → stentering → liquid ammonia.
[0120] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0121] Cold stacking: degreasing agent TF-109H: 8g / L, refining agent SA-U: 4g / L, desizing enzyme DS-HT: 6g / L, penetrant WA-M: 4g / L, caustic soda 40g / L, stacking temperature 40℃, stacking time 12h.
[0122] Oxygen bleaching: vehicle speed: 70m / min, degreasing agent TF-109H: 8g / L, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0123] Tentering: fiber protection agent PARASOFTENER CS: 20g / L, drying temperature 150℃, drying time 30s, using Monforts tentering machine.
[0124] Liquid ammonia: vehicle speed 50m / min, ammonia tank liquid level 70%, rolling rate 58%, treatment chamber temperature 65℃, steam chamber temperature 120℃, water washing tank temperature 50℃, overflow water 600L / h, using Japan Kyoto liquid ammonia finishing machine.
[0125] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0126] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0127] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0128] Using the process of Comparative Example 5, the oil spot stain score of the finished cloth was 12 points / 100 yards.
[0129] Comparative Example 6
[0130] Specifications: C / R40*C / R40*130*80*57 / 58, structure: 1 / 1, 50% cotton + 50% viscose in warp and weft, weight: 130±10g / m 2 .
[0131] Conventional process without liquid ammonia: singeing → deboiling → oxygen bleaching.
[0132] Singeing: speed 90m / min, 3#4# normal burning, flame intensity 20bar.
[0133] Deboiling: caustic soda: 40g / L, desizing enzyme DS-HT: 3g / L, penetrant WA-M: 4g / L, refining agent SA-U: 4g / L, chelating agent SQ-N: 5g / L, vehicle speed: 80m / min, steamer temperature: 98℃, piling time: 15min, PVA washing zone temperature (℃): no heating, 85, 85, 85, 85, training water washing zone temperature (℃): 95, 95, 95, 80, overflow water: 4L / kg, using Beninger deboiling machine.
[0134] Oxygen bleaching: vehicle speed: 70m / min, caustic soda (45Be): 4g / L, hydrogen peroxide (27.5%): 20g / L, chelating agent SQ-N: 10g / L, hydrogen peroxide stabilizer OUR-266: 7g / L, penetrant WA-M: 6g / L, steamer temperature: 101℃, piling time: 25min, using Beninger oxygen bleaching machine.
[0135] Conventional water washing: steamer temperature 98°C, vehicle speed 52m / min (steaming time 1 minute), washing tank temperature 50°C, overflow water 400L / h, fluorescent brightener produced by Clariant Co., Ltd. PC liq new 10g / L, caustic soda 2g / L, penetrant WA-M 1g / L, hydrogen peroxide stabilizer OUR-266 5g / L, chelating agent OUR-254 2g / L produced by Nantong Aor Industry and Trade Co., Ltd., hydrogen peroxide 15g / L, use Hongqi washing machine.
[0136] Conventional post-washing stretching: drying temperature 130℃ drying time 30s, hydrophilic silicone softener TUBINGAL MAS: 40g / L, WA-M: 2g / L produced by Tianjin Hongliyuan Company, drop width 150cm, using Monforts stenter.
[0137] Conventional preshrinking: steam drum on, tension 2kg, compression distance 8mm, rubber blanket temperature 40℃, wool blanket temperature 110℃, using Monforts preshrinking machine.
[0138] Using the process of Comparative Example 6, the finished cloth surface has no oil spots.
[0139] Note: Finished product appearance inspection standards:
[0140] 1. The four-point scoring standard for appearance defects is shown in Table 1:
[0141] Table 1
[0142] Defect size Defect review score Under 3 inches 1 point 3-6 inches 2 points 6-9 inches 3 points 9 inches to 1 meter 4 points
[0143] Note: The maximum cumulative score within 1 meter is 4 points, and all holes, regardless of size, will be scored 4 points.
[0144] 2. Scoring criteria for first-class appearance quality products:
[0145] (1) A single roll with a deduction score of less than 20 points / 100 yards is considered first-class, and a batch with a deduction score of less than 16 points / 100 yards is considered first-class;
[0146] (2) If the deduction score of a single roll is between 20 and 60 points / 100 yards, it is considered second-class product;
[0147] (3) If the deduction score for a single roll exceeds 60 points / 100 yards, it will be classified as a third-class product.
[0148] Among them, 1 yard is equal to 0.9144 meters.
[0149] The test results of Examples 1 to 3 of the present invention and Comparative Examples 1 to 6 are shown in Table 2:
[0150] Table 2
[0151]
Claims
1. A liquid ammonia pretreatment process for regenerated cellulose fiber fabric, characterized in that: Including the following processes: Singeing → cold stacking → oxygen bleaching → stentering → liquid ammonia; The cold stacking process is to roll and stack after dipping in the working solution; the working solution formula is: degreasing agent TF-109H: 4~8g / L, long-chain fatty alcohol polyoxyethylene ether refining agent: 4~8g / L, caustic soda: 30~50g / L, desizing enzyme: 4~8g / L, penetrant: 4~6g / L; The formula of the working fluid in the oxygen bleaching process is: degreasing agent TF-109H: 4~8g / L, caustic soda: 3~5g / L, hydrogen peroxide: 18~22g / L, hydrogen peroxide stabilizer: 6~8g / L, chelating agent: 8~12g / L, penetrant: 4~6g / L; The tentering process comprises padding with a fatty acid amide fiber protective agent working solution; The liquid ammonia process controls the liquid level of the liquid ammonia tank to be 30-40%, and the regenerated cellulose fiber fabric is dipped in liquid ammonia; The padding is performed to control the rolling rate to be between 75% and 80%.
2. The liquid ammonia pretreatment process for regenerated cellulose fiber fabric according to claim 1, characterized in that: The coiling and stacking temperature is 38-42°C and the time is 10-12 hours.
3. The liquid ammonia pretreatment process for regenerated cellulose fiber fabric according to claim 1, characterized in that: The drying temperature of the stentering process is 120-150°C.
4. The liquid ammonia pretreatment process for regenerated cellulose fiber fabric according to claim 3, characterized in that: The working solution concentration of the fatty acid amide fiber protective agent is 20-30 g / L.
5. The liquid ammonia pretreatment process for regenerated cellulose fiber fabric according to claim 1, characterized in that: The padding speed is 50-60 m / min.
Citation Information
Patent Citations
Production process for improving left-right color difference of dope-dyed fabric
CN114086406A
Processing method of anti-oil shirt fabric
CN114657769A
Cellulose fiber or cellulose fiber product, and method for producing them
JP2007270416A
Process for modifying regenerated cellulose fiber
US4475917A
Fibers, a process for preparing the same and product thereof
US5855624A