Copper-based bimetallic single-atom catalyst and preparation method thereof and zinc-air battery

Through the preparation of copper-based bimetallic single-atom catalysts, the problem of insufficient catalyst activity and stability in zinc-air batteries has been solved, and efficient charge and discharge cycles of zinc-air batteries have been achieved, extending battery life and reducing costs.

CN115986149BActive Publication Date: 2024-10-29TSINGHUA UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310094537.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-19
Publication Date
2024-10-29
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

During the charge and discharge process of zinc-air batteries, the oxygen reduction reaction and oxygen evolution reaction kinetics are slow and the reaction overpotential is high, which affects the overall charge and discharge cycle efficiency of zinc-air batteries. Traditional precious metal catalyst resources are scarce and expensive, and the catalysts are easy to use. Deactivation limits the large-scale application of zinc-air batteries.

Method used

Using a copper-based bimetallic single atom catalyst, the copper-based bimetallic precursor is mixed with a carrier carbon precursor and a solvent, followed by extrusion treatment, pre-oxidation and calcination, to achieve uniform distribution of copper atoms on the catalyst and improve catalytic activity and stability.

Benefits of technology

The catalytic activity and stability of the copper-based bimetallic single-atom catalyst are significantly improved, and the charge and discharge cycle life of the zinc-air battery is extended. The cycle time is more than 5,000 hours, and the number of cycles is more than 30,000 times, improving the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115986149B_ABST
    Figure CN115986149B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a copper-based bimetallic single-atom catalyst, which comprises: (1) mixing a copper-based bimetallic precursor, a carrier carbon precursor and a solvent to obtain a copper-based bimetallic single-atom catalyst precursor solution; (2) extruding the copper-based bimetallic catalyst precursor solution to obtain a copper-based bimetallic single-atom catalyst precursor; (3) pre-oxidizing the copper-based bimetallic single-atom catalyst precursor; (4) calcining the pre-oxidized copper-based bimetallic single-atom catalyst precursor under an inert atmosphere to obtain a copper-based bimetallic single-atom catalyst. Thus, the copper-based bimetallic is uniformly distributed on the copper-based bimetallic single-atom catalyst in an atomic-level manner, and the prepared copper-based bimetallic single-atom catalyst has excellent catalytic activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material synthesis and electrocatalytic battery, and specifically relates to a copper-based bimetallic single-atom catalyst and a preparation method thereof, and a zinc-air battery. Background Art

[0002] With the rapid development of industry, the excessive use of fossil fuels has caused serious environmental pollution and traditional energy shortages. The development of green energy storage and conversion technology is an inevitable choice for social development. Among the many energy storage and conversion technologies, zinc-air batteries have become the next generation of new energy storage devices with the most application potential due to their high theoretical energy density, safety, environmental friendliness, low cost, smooth discharge curve, and short recharge time. They have important application and research value.

[0003] However, there are still many problems with zinc-air batteries. For example, during the charging and discharging process of zinc-air batteries, the oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) occurring on the air cathode are both four-electron-proton coupling processes, the electrocatalytic reaction kinetics are slow, and the reaction overpotential is high, which seriously affects the overall charge and discharge cycle efficiency of zinc-air batteries and restricts the development and application of zinc-air batteries. Despite this, driven by science and technology, zinc-air batteries have certain application examples in many fields, such as hearing aids, beacon lights, wartime medical surgical lighting, etc. However, the production of its air cathode is heavily dependent on traditional precious metal-based catalysts such as Pt / C+IrO2. Due to the scarcity and high price of precious metal resources, as well as the problem of catalyst deactivation caused by poisoning during the catalytic reaction, the large-scale application of zinc-air batteries is greatly limited. Therefore, the development of non-precious metal catalyst materials with high activity, high stability and low price is of great scientific significance to the development of zinc-air batteries.

[0004] It is reported that single-atom catalysts have 100% atomic utilization, unique coordination environment, strong metal surface free energy, and exhibit high activity and high selectivity in most catalytic reactions. They are expected to replace traditional precious metal catalysts and become the first choice for a new generation of high-efficiency catalysts, and have potential application value in the field of catalysis. However, due to the high surface free energy of single atoms, in catalytic reactions, it is inevitable that metal atoms will migrate and form clusters, causing the active center to dissolve and fall off, thereby reducing the activity and stability of the catalyst, thereby affecting the battery cycle life. At the same time, people's current research on non-metallic catalysts is mainly focused on iron-based catalysts, but in ORR, a two-electron transfer process will inevitably occur to generate hydrogen peroxide, leading to the occurrence of Fenton reaction, and then deactivating the catalyst. Copper-based catalysts can avoid the occurrence of Fenton reaction, but the Cu atoms in the Cu-N4 site show a small oxygen adsorption energy and poor ORR activity, which seriously restricts its development in the field of zinc-air batteries. Therefore, developing non-precious metal single-atom copper catalysts with high stability and high activity through reasonable strategies is the key to balancing the relationship between ORR catalytic activity and durability, and is also the only way to replace traditional precious metal commercial catalysts to realize the marketization of zinc-air batteries. However, the ORR activity and stability of the currently reported single-atom copper catalysts / copper-based catalysts are still significantly different from those of precious metal catalysts. For example, the cycle stability of zinc-air batteries assembled from various material electrocatalysts does not exceed 2500 hours at most.

[0005] Therefore, there is an urgent need to further improve the intrinsic activity and stability of non-precious metal single-atom copper catalysts to achieve ultra-long charge and discharge cycle life of zinc-air batteries. Summary of the invention

[0006] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a method for preparing a copper-based bimetallic single-atom catalyst. Thus, the copper-based bimetal is uniformly distributed on the copper-based bimetallic single-atom catalyst at the atomic level, and the prepared copper-based bimetallic single-atom catalyst has good catalytic activity and stability.

[0007] In one aspect of the present invention, the present invention provides a method for preparing a copper-based bimetallic single-atom catalyst. In an embodiment of the present invention, the method comprises:

[0008] (1) mixing a copper-based bimetallic precursor, a carrier carbon precursor and a solvent to obtain a copper-based bimetallic single-atom catalyst precursor solution;

[0009] (2) extruding the copper-based bimetallic catalyst precursor solution to obtain a copper-based bimetallic single-atom catalyst precursor;

[0010] (3) pre-oxidizing the copper-based bimetallic single-atom catalyst precursor;

[0011] (4) Under an inert atmosphere, calcining the pre-oxidized copper-based bimetallic single-atom catalyst precursor to obtain a copper-based bimetallic single-atom catalyst.

[0012] According to the method for preparing a copper-based bimetallic single-atom catalyst according to an embodiment of the present invention, the copper-based bimetallic is uniformly distributed on the copper-based bimetallic single-atom catalyst obtained in the present application in an atomic-level manner, and the copper atom utilization rate of the copper-based bimetallic single-atom catalyst reaches the maximum atomic utilization rate of copper (100%). Due to the activation effect of the main group metal atoms on the single-atom copper sites, the copper-based bimetallic single-atom catalyst has good oxygen reduction reaction and oxygen evolution reaction activity and stability under alkaline conditions. In particular, when the copper-based bimetallic single-atom catalyst is used as an electrode catalyst for ORR reaction, it has excellent ORR catalytic activity and stability.

[0013] In addition, the method according to the above embodiment of the present invention may also have the following additional technical features:

[0014] In some embodiments of the present invention, in step (2), the extrusion processing method includes at least one of solution air spinning, electrospinning and 3D printing, preferably solution air spinning.

[0015] In some embodiments of the present invention, the copper-based bimetallic single-atom catalyst precursor obtained by the extrusion process has a shape including at least one of fibrous, tubular, and bamboo-like, preferably fibrous.

[0016] In some embodiments of the present invention, step (1) further comprises:

[0017] (1-1) mixing the copper-based bimetallic precursor and the solvent to obtain a copper-based bimetallic precursor mixed solution;

[0018] (1-2) Mixing the copper-based bimetallic precursor mixed solution and the carrier carbon precursor to obtain the copper-based bimetallic single-atom catalyst precursor solution.

[0019] In some embodiments of the present invention, the copper-based bimetallic precursor is a mixture of sodium copper chlorophyllin or a copper phthalocyanine complex and sodium chloride.

[0020] In some embodiments of the present invention, the carrier carbon precursor includes at least one of polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polystyrene and polyamide, preferably polyacrylonitrile.

[0021] In some embodiments of the present invention, the solvent includes at least one of N,N-dimethylformamide, dimethyl sulfoxide, sulfolane, and ethyl nitrate, preferably N,N-dimethylformamide.

[0022] In some embodiments of the present invention, the mass ratio of the copper-based bimetallic precursor to the carrier carbon precursor is (5-30):100, preferably (15-20):100.

[0023] In some embodiments of the present invention, the mass ratio of the solvent to the carrier carbon precursor is (5-12):1, preferably (9-12):1.

[0024] In some embodiments of the present invention, step (3) further comprises:

[0025] The copper-based bimetallic single-atom catalyst precursor is dried before the pre-oxidation treatment.

[0026] In some embodiments of the present invention, in step (3), the pre-oxidation temperature is 200-280°C, preferably 220-260°C.

[0027] In some embodiments of the present invention, the pre-oxidation time is 0.5 to 3 hours, preferably 2 to 3 hours.

[0028] In some embodiments of the present invention, in step (4), the calcination temperature is 500-950°C, preferably 800-900°C.

[0029] In some embodiments of the present invention, the calcination time is 1 to 3 hours, preferably 1.5 to 2 hours.

[0030] In another aspect of the present invention, the present invention provides a copper-based bimetallic single-atom catalyst. According to an embodiment of the present invention, the copper-based bimetallic single-atom catalyst is prepared by the method for preparing the copper-based bimetallic single-atom catalyst described in the above embodiment. Thus, the catalytic activity and stability of the copper-based bimetallic single-atom catalyst are significantly improved.

[0031] In the third aspect of the present invention, the present invention provides a zinc-air battery. According to an embodiment of the present invention, the zinc-air battery has a copper-based bimetallic single-atom catalyst prepared by the method described in the above embodiment or the copper-based bimetallic single-atom catalyst described in the above embodiment. Therefore, due to the addition of the above copper-based bimetallic single-atom catalyst, the charge and discharge cycle time of the zinc-air battery is greater than 5000 hours; the number of charge and discharge cycles of the zinc-air battery is greater than 30000 times.

[0032] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0034] Figure 1 is a flow chart of a method for preparing a copper-based bimetallic single-atom catalyst according to an embodiment of the present invention;

[0035] Figure 2 This is a schematic diagram of the molecular structure of sodium copper chlorophyllin according to an embodiment of the present invention:

[0036] Figure 3 A schematic diagram of a flow chart of a method for preparing a copper-based bimetallic single-atom catalyst according to an embodiment of the present invention;

[0037] Figure 4 This is a SEM image of the copper-sodium bimetallic single-atom catalyst prepared in Example 1;

[0038] Figure 5 TEM image of the copper-sodium bimetallic single atom catalyst prepared in Example 1;

[0039] Figure 6 The XRD patterns of the catalysts prepared in Example 1, Example 2 and Comparative Example 1;

[0040] Figure 7 HAADF-STEM images of the catalysts prepared in Example 1 and Comparative Example 1;

[0041] Figure 8 are XAFS graphs of the catalysts prepared in Example 1 and Comparative Example 1; wherein Figure (a) is an X-ray absorption near-edge structure graph of the catalysts prepared in Example 1 and Comparative Example 1, Figure (b) is an extended X-ray absorption fine structure graph and a structure fitting graph of the catalyst prepared in Example 1, and Figure (c) is an extended X-ray absorption fine structure graph and a structure fitting graph of the catalyst prepared in Comparative Example 1;

[0042] Fig. 9 Linear sweep voltammetric characteristic curve of electrocatalytic ORR using the catalysts prepared in Examples 1 to 6 as electrode catalysts;

[0043] Fig.10 Linear sweep voltammetric characteristic curves of the catalysts prepared in Comparative Examples 1 to 4 as electrode catalysts for electrocatalytic ORR;

[0044] Fig.11DFT theoretical calculations corresponding to electrocatalytic ORR of the catalysts prepared in Example 1 and Comparative Example 1 as electrode catalysts; (a) is the reaction path of the catalyst prepared in Example 1 when performing ORR, (b) is the reaction path of the catalyst prepared in Comparative Example 1 when performing ORR, (c) oxygen adsorption energy analysis of the catalysts prepared in Example 1 and Comparative Example 1 in ORR reaction;

[0045] Fig.12 The ORR stability chronoamperometric curves are obtained by using the catalysts prepared in Example 1 and Comparative Example 4 as working electrodes;

[0046] Fig.13 The OER linear sweep voltammetric characteristic curves are obtained by using the catalysts prepared in Example 1, Example 2, Comparative Examples 1 to 3, and Comparative Example 5 as working electrodes;

[0047] Fig.14 The OER stability potential-time curves of the catalysts prepared in Example 1 and Comparative Example 5 as working electrodes;

[0048] Fig.15 The catalyst prepared in Example 1 is assembled into a liquid zinc-air battery and the cycle stability curve is at a current of 10 mA;

[0049] Fig.16 The catalyst prepared in Comparative Example 4 is assembled into a liquid zinc-air battery and the cycle stability curve at a current of 10 mA;

[0050] Fig.17 The cyclic stability curve of the liquid zinc-air battery assembled with the catalyst prepared in Example 1 at a current of 1 mA;

[0051] Fig.18 The cyclic stability curve of the catalyst prepared in Example 1 assembled into a flexible zinc-air battery at a current of 1 mA;

[0052] Fig.19 This is the cycle stability curve of a button-type zinc-air battery assembled with the catalyst prepared in Example 1 at a current of 10 mA. Specific implementation methods

[0053] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0054] The present invention provides a method for preparing a copper-based bimetallic single-atom catalyst. Figure 1 , the above method comprises:

[0055] S100: Mixing a copper-based bimetallic precursor, a carrier carbon precursor and a solvent to obtain a copper-based bimetallic single-atom catalyst precursor solution

[0056] In this step, a copper-based bimetallic precursor, a carrier carbon precursor and a solvent are mixed to obtain a copper-based bimetallic single-atom catalyst precursor solution.

[0057] In an embodiment of the present invention, in step S100, the type of copper-based bimetallic precursor is not particularly limited, and those skilled in the art may select it according to actual needs. As a specific example, the copper-based bimetallic precursor may be a mixture of sodium copper chlorophyllin or a copper phthalocyanine complex and sodium chloride.

[0058] According to a specific embodiment of the present invention, in step S100, the bimetallic complex is sodium copper chlorophyllin, and the molecular structure of sodium copper chlorophyllin is as shown in the attached Figure 2 As shown, there are two metal elements, copper and sodium, in the sodium copper chlorophyllin salt, with an atomic ratio of 1:3, which ensures that the copper atoms and sodium atoms in the obtained copper-sodium bimetallic single atom catalyst have a good doping effect; at the same time, the molecular structure of the sodium copper chlorophyllin salt has the molecular structure characteristics of a benzene ring, the copper atom is connected to the four surrounding nitrogen atoms, and the sodium atom is fixed by the carboxylate. The benzene ring-like molecular structure around the copper atom can form steric hindrance to a certain extent, preventing the copper atoms from agglomerating in subsequent treatments to produce nanoparticles, which is beneficial to the effective synthesis of the sodium copper bimetallic single atom catalyst.

[0059] According to another specific embodiment of the present invention, in step S100, the mass ratio of the copper phthalocyanine complex and sodium chloride is (2-4): 1. Thus, by controlling the mass ratio of the copper phthalocyanine complex and sodium chloride within the above range, the doping amount of metallic copper and sodium in the final catalyst can be ensured, which is beneficial to the ORR activation of copper atoms by sodium and improves the intrinsic activity and stability of the catalyst.

[0060] In an embodiment of the present invention, in step S100, the type of the carrier carbon precursor is not particularly limited, and those skilled in the art may select it according to actual needs. As a specific example, the carrier carbon precursor includes at least one of polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polystyrene and polyamide.

[0061] Preferably, in step S100, the carrier carbon precursor is polyacrylonitrile. Compared with other commonly used carrier carbon precursors (such as polyvinyl alcohol, polyvinyl pyrrolidone, polystyrene and polyamide), polyacrylonitrile (PAN) has the advantages of high carbonization yield and good flexibility. In the subsequent carbonization process (calcination process), atoms other than carbon are difficult to affect and destroy the skeleton structure of polyacrylonitrile, which is conducive to the dispersion of copper-based bimetallics.

[0062] In an embodiment of the present invention, in step S100, the type of solvent is not particularly limited, and those skilled in the art may select the solvent according to actual needs. As a specific example, at least one of the above-mentioned solvents N,N-dimethylformamide, dimethyl sulfoxide, cyclopentane sulfone, and ethyl nitrate is preferably N,N-dimethylformamide.

[0063] According to another specific embodiment of the present invention, in step S100, the mass ratio of the above-mentioned copper-based bimetallic precursor and the above-mentioned carrier carbon precursor is (5-30):100, preferably (15-20):100. Thus, the mass ratio of the above-mentioned copper-based bimetallic precursor and the above-mentioned carrier carbon precursor is controlled within the above-mentioned range, which can not only ensure that the subsequently obtained copper-based bimetallic single-atom catalyst has a good bimetallic loading, thereby improving the catalytic activity of the copper-based bimetallic single-atom catalyst, but also obtain a copper-based bimetallic single-atom catalyst precursor solution with good viscosity and fluidity, which is beneficial to the subsequent extrusion treatment of the copper-based bimetallic catalyst precursor solution.

[0064] According to another specific embodiment of the present invention, in step S100, the mass ratio of the above-mentioned solvent to the above-mentioned carrier carbon precursor is (5-12):1, preferably (9-12):1. Therefore, the above-mentioned mass ratio of the above-mentioned carrier carbon precursor and the solvent is controlled within the above-mentioned range, which can not only ensure that the subsequently obtained copper-based bimetallic single-atom catalyst has a good bimetallic loading, thereby improving the catalytic activity of the copper-based bimetallic single-atom catalyst, but also obtain a copper-based bimetallic single-atom catalyst precursor solution with good viscosity and fluidity, which is beneficial to the subsequent extrusion treatment of the copper-based bimetallic catalyst precursor solution.

[0065] According to another specific embodiment of the present invention, step S100 further includes:

[0066] S101: Mixing the copper-based bimetallic precursor and the solvent to obtain a copper-based bimetallic precursor mixed solution.

[0067] In an embodiment of the present invention, in step S101, the method for mixing the copper-based bimetallic precursor and the solvent is not particularly limited, and those skilled in the art may select the method according to actual needs. As a specific example, the method for mixing the copper-based bimetallic precursor and the solvent may be at least one of ultrasonic mixing and magnetic stirring.

[0068] According to another specific embodiment of the present invention, in step S101, the copper-based bimetallic precursor and the solvent are first ultrasonically mixed, and the ultrasonic time is 10 to 30 minutes. The ultrasonic power is not particularly limited and can be adjusted according to actual conditions; then the mixed liquid after ultrasonic mixing is magnetically stirred, and the magnetic stirring speed is 300 to 600 rpm, and the magnetic stirring time is 6 to 24 hours, so as to achieve uniform distribution of the copper-based bimetallic precursor in the solvent.

[0069] S102: Mixing the copper-based bimetallic precursor mixture and the carrier carbon precursor to obtain the copper-based bimetallic single-atom catalyst precursor solution.

[0070] In an embodiment of the present invention, in step S102, the method for mixing the copper-based bimetallic precursor mixed liquid and the carrier carbon precursor is not particularly limited, and those skilled in the art may select it according to actual needs. As a specific example, the method for mixing the copper-based bimetallic precursor mixed liquid and the carrier carbon precursor may be magnetic stirring.

[0071] According to another specific embodiment of the present invention, in step S102, the copper-based bimetallic precursor mixed liquid and the carrier carbon precursor are magnetically stirred and mixed, the rotation speed of the magnetic stirring is 300 to 500 rpm, and the time of the magnetic stirring is 24 to 48 hours, so as to achieve sufficient mixing of the copper-based bimetallic precursor mixed liquid and the carrier carbon precursor.

[0072] Therefore, by adopting the step-by-step dispersion method, the copper-based bimetallic precursor and the solvent can be fully mixed to form a copper-based bimetallic precursor mixed liquid, and the copper-based bimetallic precursor mixed liquid is then mixed with a carrier carbon precursor to obtain a copper-based bimetallic single-atom catalyst precursor solution, which significantly improves the mixing efficiency and the utilization rate of the copper-based bimetallic precursor, the carrier carbon precursor and the solvent.

[0073] S200: Extruding the copper-based bimetallic catalyst precursor solution to obtain a copper-based bimetallic single-atom catalyst precursor

[0074] In this step, the copper-based bimetallic catalyst precursor solution is extruded to obtain a copper-based bimetallic single-atom catalyst precursor, which is beneficial to increase the specific surface area of ​​the copper-based bimetallic single-atom catalyst precursor, and further beneficial to improve the catalytic activity and stability of the subsequently obtained copper-based bimetallic single-atom catalyst.

[0075] In an embodiment of the present invention, in step S200, the extrusion processing method is not particularly limited, and those skilled in the art may select it according to actual needs. As a specific example, the extrusion processing method includes at least one of solution air spinning, electrospinning and 3D printing, and the solution air spinning method is preferred.

[0076] According to another specific embodiment of the present invention, refer to the attached Figure 3 In step S200, the method for extruding the copper-based bimetallic catalyst precursor solution is a solution gas spinning method. Most of the copper-based bimetallic single-atom catalyst precursors obtained by the solution gas spinning method have a fibrous structure. The fibrous copper-based bimetallic single-atom catalyst precursor has a relatively smooth outer surface, and the thickness of the fibrous copper-based bimetallic single-atom catalyst precursor is uniform. In addition, compared with traditional extrusion technology (electrospinning and 3D printing), the solution gas spinning method has the characteristics of ultra-high polymer injection rate, low cost, environmental friendliness, safety and convenience, and has become the most promising technology for industrial production of micro-nano fiber structures. Therefore, mass production of copper-based bimetallic single-atom catalysts can be achieved, and it has the advantages of mild preparation conditions and safe preparation process.

[0077] According to another specific embodiment of the present invention, in step S200, the solution air spinning syringe needle model in the above-mentioned solution air spinning technology is 13G~34G, preferably 20~32G; the release rate of the copper-based bimetallic catalyst precursor solution at the solution air spinning syringe needle is 0.8~1.2mL / h, preferably 0.9~1.1mL / h; the high-speed air jet flow rate around the solution air spinning syringe needle is 30~60L / min, preferably 40~50L / min; the distance between the non-woven fabric used to collect the fibrous copper-based bimetallic single-atom catalyst precursor and the solution air spinning syringe needle tip is 25~35cm, thereby, a fibrous copper-based bimetallic single-atom catalyst precursor with uniform thickness and smooth surface can be obtained.

[0078] According to another specific embodiment of the present invention, in step S200, the shape of the copper-based bimetallic single atom catalyst precursor obtained by completing the above-mentioned extrusion treatment includes at least one of fibrous, tubular, and bamboo-shaped, preferably fibrous. The fibrous copper-based bimetallic single atom catalyst precursor has the advantages of uniform thickness and consistent length. The diameter of the fibrous copper-based bimetallic single atom catalyst precursor is generally 230 to 250 nm.

[0079] S300: Pre-oxidation of copper-based bimetallic single-atom catalyst precursors

[0080] In this step, refer to the attached Figure 3 , pre-oxidation of the copper-based bimetallic single atom catalyst precursor is beneficial to stabilizing the copper-based bimetallic precursor.

[0081] For example, when the copper-based bimetallic precursor is sodium copper chlorophyll, during the pre-oxidation process of the copper-based bimetallic single-atom catalyst precursor, the linear structure of the carrier carbon precursor (such as polyacrylonitrile molecule) will be converted into a pre-oxidation material with a heat-resistant aromatic ladder structure, and at the same time, the sodium copper chlorophyll complex will combine with the aromatic ring structure formed by the pre-oxidation of the polyacrylonitrile molecule, and the sodium copper chlorophyll complex will enter the aromatic ring plane formed by the pre-oxidation of the polyacrylonitrile molecule. The aromatic ring structure in the sodium copper chlorophyll complex will form a π-π interaction with the upper and lower benzene rings formed by the pre-oxidation of the polyacrylonitrile molecule, thereby further stabilizing the sodium copper chlorophyll complex.

[0082] It should be noted that the other carrier carbon precursors play a similar role to the above-mentioned polyacrylonitrile in this application, and will not be described in detail here.

[0083] According to another specific embodiment of the present invention, step S300 also includes: drying the above-mentioned copper-based bimetallic single-atom catalyst precursor before pre-oxidation treatment, thereby removing the solvent on the surface of the copper-based bimetallic single-atom catalyst precursor, which is conducive to better pre-oxidation of the copper-based bimetallic single-atom catalyst precursor.

[0084] In an embodiment of the present invention, in step S300, the method of drying the above-mentioned copper-based bimetallic single-atom catalyst precursor before pre-oxidation treatment is not particularly limited, and those skilled in the art can choose according to actual needs. As a specific example, the method of drying the above-mentioned copper-based bimetallic single-atom catalyst precursor before pre-oxidation treatment is oven drying.

[0085] According to another specific embodiment of the present invention, an oven is used to dry the above-mentioned copper-based bimetallic single-atom catalyst precursor before pre-oxidation treatment. The oven temperature is 40-80°C, preferably 50-60°C. There is no special restriction on the drying time. It is only necessary to confirm that there is no large amount of solvent residue in the dried copper-based bimetallic single-atom catalyst precursor. This ensures that the pre-oxidized copper-based bimetallic single-atom catalyst precursor will not stick together and can maintain a better solid structure.

[0086] According to another specific embodiment of the present invention, in step S300, the pre-oxidation temperature is 200-280°C; preferably 220-260°C. Thus, controlling the pre-oxidation temperature within the above range is beneficial to improving the flexibility of the pre-oxidized copper-based bimetallic single-atom catalyst precursor, thereby improving the flexibility of the subsequently obtained copper-based bimetallic single-atom catalyst.

[0087] According to another specific embodiment of the present invention, in step S300, the pre-oxidation time is 0.5 to 3 hours, preferably 2 to 3 hours. Therefore, controlling the pre-oxidation time within the above range is beneficial to improving the flexibility of the copper-based bimetallic single-atom catalyst precursor after pre-oxidation, and further improving the flexibility of the subsequently obtained copper-based bimetallic single-atom catalyst.

[0088] S400: Under an inert atmosphere, calcining the pre-oxidized copper-based bimetallic single-atom catalyst precursor to obtain a copper-based bimetallic single-atom catalyst

[0089] In this step, refer to the attached Figure 3 , under an inert atmosphere, the pre-oxidized copper-based bimetallic single-atom catalyst precursor is calcined to obtain a copper-based bimetallic single-atom catalyst.

[0090] For example, when the copper-based bimetallic precursor is sodium copper chlorophyllin, during the calcination of the pre-oxidized copper-based bimetallic single-atom catalyst precursor, the sodium copper chlorophyllin complex will partially decompose and enter the carbon lattice formed by the carbonization of the carrier carbon precursor. The copper atom is connected to four nitrogen atoms and to two adjacent carbons in the lower carbon lattice, thereby forming a hexacoordinate configuration with a coordination mode of CuN4C2.

[0091] Furthermore, the direct bonding of copper atoms with carbon atoms in the lower aromatic plane can greatly improve the conductivity and stability of copper-based bimetallic single atom catalysts. Under high temperature conditions, sodium carboxylates will partially decompose, and there is obvious charge transfer between sodium carboxylates and copper single atoms, which is beneficial to adjust the electronic structure of the active site of the catalyst CuN4, and is beneficial to the adsorption and activation of oxygen by copper-based bimetallic single atom catalysts in ORR, thereby improving the activity and stability of copper-based bimetallic single atom catalysts. Finally, the ratio of copper atoms to sodium atoms on the copper-based bimetallic single atom catalyst is 1:1. As a result, the copper-sodium bimetallic atoms are evenly distributed on the copper-based bimetallic single atom catalyst, and the prepared copper-sodium bimetallic single atom catalyst has excellent catalytic activity and stability.

[0092] According to another specific embodiment of the present invention, step S400 also includes: cooling the calcined copper-based bimetallic single-atom catalyst to room temperature, thereby avoiding oxidation of the copper-based bimetallic single-atom catalyst, and further obtaining a copper-based bimetallic single-atom catalyst with good flexibility. The copper-based bimetallic single-atom catalyst with good flexibility can directly carry out subsequent electrocatalytic reactions and battery tests.

[0093] According to another specific embodiment of the present invention, in step S400, the inert gas used in the inert atmosphere is nitrogen, and the purity of the nitrogen is not less than 99.9999%. Thus, the purity of the nitrogen is controlled within the above range, ensuring that no new heteroatoms are introduced during the calcination process.

[0094] According to another specific embodiment of the present invention, in step S400, the calcination temperature is 500-950°C, preferably 800-900°C. Thus, the calcination temperature is controlled within the above range, which ensures that the copper-based bimetallic single-atom catalyst precursor can be carbonized and avoids the copper-based bimetallic from agglomerating into nano-metal particles, thereby maintaining the single-atom state.

[0095] According to another specific embodiment of the present invention, in step S400, the calcination time is 1 to 3 hours, preferably 1.5 to 2 hours. Thus, the calcination time is controlled within the above range, which ensures the carbonization of the copper-based bimetallic single-atom catalyst precursor and prevents the copper-based bimetal from agglomerating into nano-metal particles, thereby maintaining the single-atom state.

[0096] According to another specific embodiment of the present invention, using a copper-based bimetallic single-atom catalyst as an electrocatalytic electrode to carry out an ORR reaction can drive the ORR to occur at a smaller overpotential and have excellent ORR stability.

[0097] According to another specific embodiment of the present invention, using a copper-based bimetallic single-atom catalyst as an electrocatalytic electrode to carry out an OER reaction can achieve 10 mA cm at a lower potential. -2 The current density is high and the OER stability is excellent.

[0098] According to the method for preparing a copper-based bimetallic single-atom catalyst according to an embodiment of the present invention, a copper-based bimetallic precursor, a carrier carbon precursor and a solvent are mixed to obtain a catalyst precursor solution containing a copper-based bimetallic; the copper-based bimetallic catalyst precursor solution is subjected to an extrusion treatment, which is beneficial to increasing the surface area of ​​the copper-based bimetallic single-atom catalyst precursor, and further beneficial to improving the catalytic activity of the subsequently obtained copper-based bimetallic single-atom catalyst; the copper-based bimetallic single-atom catalyst precursor is pre-oxidized, which is beneficial to stabilizing the copper-based bimetallic precursor; under an inert atmosphere, the pre-oxidized copper-based bimetallic single-atom catalyst precursor is calcined, which is beneficial to forming a stable copper-based bimetallic single-atom catalyst structure.

[0099] At the same time, the copper-based bimetallic is uniformly distributed on the copper-based bimetallic single-atom catalyst obtained in the present application in an atomic-level manner, and the copper atom utilization rate of the copper-based bimetallic single-atom catalyst reaches the maximum copper atomic utilization rate (100%). Due to the activation effect of the main group metal atoms on the single-atom copper site, the copper-based bimetallic single-atom catalyst has good oxygen reduction reaction and oxygen evolution reaction activity and stability under alkaline conditions, especially when the copper-based bimetallic single-atom catalyst is used as an electrode catalyst for the ORR reaction, it has excellent ORR catalytic activity and stability. Thus, the copper-based bimetallic is uniformly distributed on the copper-based bimetallic single-atom catalyst in an atomic-level manner, and the prepared copper-based bimetallic single-atom catalyst has good catalytic activity and stability.

[0100] In another aspect of the present invention, the present invention provides a copper-based bimetallic single-atom catalyst. According to an embodiment of the present invention, the copper-based bimetallic single-atom catalyst is prepared by the method for preparing the copper-based bimetallic single-atom catalyst described in the above embodiment. Thus, the catalytic activity and stability of the copper-based bimetallic single-atom catalyst are significantly improved.

[0101] In the third aspect of the present invention, the present invention provides a zinc-air battery. According to an embodiment of the present invention, the zinc-air battery has a copper-based bimetallic single-atom catalyst prepared by the method described in the above embodiment or the copper-based bimetallic single-atom catalyst described in the above embodiment. Due to the addition of the copper-based bimetallic single-atom catalyst, the charge and discharge cycle time of the zinc-air battery is greater than 5,000 hours, and the number of charge and discharge cycles of the zinc-air battery is greater than 30,000 times, thereby significantly improving the cycle stability of the assembled zinc-air battery and greatly increasing the charge and discharge cycle life of the zinc-air battery.

[0102] According to another specific embodiment of the present invention, the zinc-air battery includes at least one of a liquid zinc-air battery, a flexible zinc-air battery, and a button-type zinc-air battery.

[0103] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0104] Example 1

[0105] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst, the steps of which are as follows:

[0106] (1) 0.1709 g of sodium copper chlorophyllin and 10.0 mL (9.48 g) of N,N-dimethylformamide solvent were ultrasonically mixed for 30 min, and the mixed solution after ultrasonic mixing was magnetically stirred to obtain a sodium copper bimetallic precursor mixed solution, the speed of magnetic stirring was 500 rpm, and the time of magnetic stirring was 24 h; the copper-based bimetallic precursor mixed solution and 1.0000 g of polyacrylonitrile-supported carbon precursor were magnetically stirred to obtain a green sodium copper bimetallic single-atom catalyst precursor solution with certain fluidity, the speed of magnetic stirring was 500 rpm, and the time of magnetic stirring was 48 h;

[0107] (2) The green copper-sodium bimetallic single-atom catalyst precursor solution is transferred into a 3 mL syringe with a 30G needle, and a fibrous copper-sodium bimetallic single-atom catalyst precursor is prepared by solution air spinning technology; during the solution blowing process, the spinning solution injection rate in the syringe is set to 1.00 mL / h, the high-speed air jet around the syringe needle is set to 45.00 L / min, and the distance between the nozzle tip and the non-woven fabric collector is set to 35 cm. The fibrous copper-sodium bimetallic single-atom catalyst precursor obtained by the solution air spinning technology is placed in a vacuum oven at 60° C. and dried until it is observed that there is no large amount of solvent residue in the dried copper-sodium bimetallic single-atom catalyst precursor;

[0108] (3) pre-oxidizing the copper-sodium bimetallic single-atom catalyst precursor, the pre-oxidation device is a constant temperature forced air drying oven, the pre-oxidation temperature is 260° C., the pre-oxidation time is 3 h, and the heating rate is set to 1° C. / min;

[0109] (4) The pre-oxidized copper-sodium bimetallic single-atom catalyst precursor is calcined under a 100 sccm flow of 99.9999% high-purity argon gas. The temperature is first increased to 900°C at a heating rate of 5°C / min, the calcination temperature is 900°C, and the calcination time is 2h. The calcined copper-sodium bimetallic single-atom catalyst is then cooled to room temperature to obtain the copper-sodium bimetallic single-atom catalyst.

[0110] Example 2

[0111] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst. The difference between this embodiment and embodiment 1 is only that:

[0112] The sodium copper chlorophyllin was replaced by a mixture of a copper phthalocyanine complex not containing sodium and sodium chloride. The mass of the copper phthalocyanine complex not containing sodium was 0.1360 g, and the mass of the sodium chloride was 0.0414 g.

[0113] Example 3

[0114] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst. The difference between this embodiment and embodiment 1 is only that:

[0115] The amount of sodium copper chlorophyllin added is 0.0570g.

[0116] Example 4

[0117] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst. The difference between this embodiment and embodiment 1 is only that:

[0118] The amount of sodium copper chlorophyllin added is 0.285g.

[0119] Example 5

[0120] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst. The difference between this embodiment and embodiment 1 is only that:

[0121] The calcination temperature is 750°C.

[0122] Example 6

[0123] This embodiment provides a method for preparing a copper-sodium bimetallic single-atom catalyst. The difference between this embodiment and embodiment 1 is only that:

[0124] The calcination temperature is 950°C.

[0125] Comparative Example 1

[0126] This comparative example provides a method for preparing a catalyst. The difference between this comparative example and Example 1 is only that:

[0127] The sodium copper chlorophyllin was replaced by a copper phthalocyanine complex that does not contain sodium.

[0128] Comparative Example 2

[0129] This comparative example provides a method for preparing a catalyst. The difference between this comparative example and Example 1 is only that:

[0130] Replace the sodium copper chlorophyllin with sodium chloride.

[0131] Comparative Example 3

[0132] This comparative example provides a method for preparing a catalyst. The difference between this comparative example and Example 1 is only that:

[0133] Step (1) removes the metal precursor and only mixes the carrier carbon precursor and the solvent.

[0134] Comparative Example 4

[0135] The commercial Pt / C catalyst with a Pt loading of 20 wt% was directly used to replace the copper-sodium bimetallic single atom catalyst.

[0136] Comparative Example 5

[0137] The commercial IrO2·xH2O catalyst with an Ir loading of 73 wt% was directly used to replace the CuNa bimetallic single atom catalyst.

[0138] The copper-sodium bimetallic single-atom catalyst of Example 1 was subjected to scanning electron microscopy to obtain a SEM image of the copper-sodium bimetallic single-atom catalyst, as shown in the attached figure. Figure 4 The copper-sodium bimetallic single-atom catalyst of Example 1 was subjected to transmission electron microscopy to obtain a TEM image of the copper-sodium bimetallic single-atom catalyst, as shown in the attached figure. Figure 5 As shown in the attached Figure 4 and attached Figure 5 It can be seen that the surface of the fibrous copper-sodium bimetallic single atom material prepared in Example 1 is relatively smooth, and the fiber diameter is about 220 nm.

[0139] The catalysts prepared in Example 1, Example 2 and Comparative Example 1 were subjected to XRD detection to obtain XRD spectra, wherein Cu JCPDS#04-0836 is a standard XRD spectrum of copper. Figure 6 It can be seen that there is no characteristic peak of copper in the XRD spectra of the catalysts prepared in Example 1, Example 2 and Comparative Example 1, and copper is dispersed in the prepared catalysts in the form of atoms.

[0140] The catalysts prepared in Example 1 and Comparative Example 1 were subjected to high-angle annular dark field scanning transmission electron microscopy to obtain HAADF-STEM images. Figure 7It can be seen that the copper atoms of the catalysts prepared in Example 1 and Comparative Example 1 are evenly dispersed, and no copper nanoparticles exist.

[0141] The catalysts prepared in Example 1 and Comparative Example 1 were subjected to X-ray absorption fine structure spectrum analysis to obtain XAFS graphs. Figure 8 (a) It can be seen that by comparing the X-ray absorption near-edge structure diagram of the copper foil with a copper valence of 0 and the copper oxide material with a copper valence of +2, it can be obtained that the valence of copper in Example 1 and Comparative Example 1 is between 0 and +2. Figure 8 (b) and Figure 8 (c) It can be seen that the characteristic peak of Cu-Cu coordination bond does not appear in the extended X-ray absorption fine structure spectra of Example 1 and Comparative Example 1, which proves that there is no Cu-Cu bond in the catalysts prepared in Example 1 and Comparative Example 1, and copper exists in the catalysts prepared in Example 1 and Comparative Example 1 in the form of atomic dispersion. Through fitting, it is determined that the Cu coordination environment in the catalysts prepared in Example 1 and Comparative Example 1 is CuN4C2-(COONa) and CuN4C2, respectively. The coordination of Cu-C2 in the catalysts prepared in Example 1 and Comparative Example 1 proves the active site carbon coating and the bonding structure between copper and the carrier formed during the synthesis of the two catalysts, which is of great significance to the stability of the electrochemical reaction.

[0142] A 0.1 mol / L potassium hydroxide aqueous solution was used as the electrolyte, and a conventional three-electrode configuration (graphite rod as the counter electrode, Ag / AgCl (3.5 M KCl) electrode as the reference electrode, and a loading of 0.2 mg / cm 2 The ORR electrocatalytic test was carried out on an electrochemical workstation using the rotating disk electrode of the catalysts prepared in Examples 1-6 and Comparative Examples 1 to 4 as the working electrode, and a linear scanning voltammetric curve was obtained at a scanning rate of 5 mV / s, as shown in the attached figure. Fig. 9 and attached Fig.10As shown, the electrocatalytic ORR activity of the catalysts prepared in Examples 1-6 as electrode catalysts is significantly better than that of Comparative Examples 1-3; by comparing Examples 1-6 and Comparative Examples 1-3, it is proved that the introduction of metallic sodium into the pure carbon precursor material has a certain effect on improving the ORR activity of the catalyst; and when copper metal single atoms are introduced into the pure carbon precursor material, the ORR activity can be effectively improved; when copper and sodium bimetallics are simultaneously introduced into the pure carbon precursor material, due to the synergistic effect of the bimetallics, the catalytic activity of the bimetallics is significantly better than the catalytic activity of the catalyst prepared from the pure carbon precursor material doped with copper / sodium single metals; when the bimetallic doping forms the specific active site CuN4-(COONa) in Examples 1-6, the ORR performance of the prepared catalyst reaches the best; in addition, the electrocatalytic ORR activity of the catalyst prepared in Example 1 as an electrode catalyst is higher than the ORR activity of the precious metal catalyst (commercial Pt / C catalyst with a Pt loading of 20wt%) in Comparative Example 4, and the ORR activity of the catalysts prepared in Examples 2-6 is equivalent to that of the precious metal catalyst in Comparative Example 4.

[0143] In order to further reveal the significance of CuN4-(COONa) to ORR activity, the reaction pathway and oxygen adsorption energy of CuN4-(COONa) in Example 1 and CuN4 in Comparative Example 1 during ORR were analyzed by DFT theoretical calculation. Fig.11 As shown, the rate controlling step of ORR of the catalysts prepared in Example 1 and Comparative Example 1 is the adsorption and activation process of oxygen on the active site. In Example 1, due to the charge transfer effect between CuN4 and the adjacent COONa functional group, the oxygen adsorption energy is more negative, which is beneficial to the adsorption and activation of oxygen on the active site, resulting in the catalyst prepared in Example 1 having high ORR activity.

[0144] In the ORR stability test, the chronoamperometric curves of the catalysts prepared in Example 1 and Comparative Example 4 at a potential of 0.7 V were tested respectively. Fig.12 As shown, the catalyst prepared by the copper-sodium bimetallic single atom doped carbon fiber provided by the present invention can maintain a constant electrode current of 99.91% after a long period of electrocatalytic oxygen reduction reaction, which is significantly better than the commercial Pt / C catalyst corresponding to Comparative Example 4. The ultra-high ORR stability of the catalyst prepared in Example 1 is due to the specific active site carbon coating and the specific CuN4C2-(COONa) structure formed during the synthesis of the prepared catalyst.

[0145] A 1.0 mol / L potassium hydroxide aqueous solution was used as the electrolyte, and a conventional three-electrode configuration (graphite rod as the counter electrode, Ag / AgCl (3.5 M KCl) electrode as the reference electrode, and a loading of 0.2 mg / cm 2 The OER electrocatalytic test was carried out on an electrochemical workstation using the carbon cloth of Examples 1 to 2, Comparative Examples 1 to 3 and Comparative Example 5 as the working electrode. A linear sweep voltammetric curve was obtained at a scan rate of 10 mV / s, as shown in Fig.13 As shown in the figure, the electrocatalytic OER activity of the catalyst prepared in Example 1-2 as an electrode catalyst is significantly better than the OER activity of Comparative Examples 1-3, indicating that the catalyst prepared in Example 1-2 has excellent electrocatalytic OER performance. The "chronopotentiometry" method was used, and the current density was set to 10 mA cm -2 The corresponding current was measured by performing a chronopotentiometry test on the electrodes assembled from the materials of Example 1 and Comparative Example 5 for 10 hours. The potential-time curve is shown in FIG. Fig.14 As shown. Fig.14 It can be seen that the catalyst prepared in Example 1 has a -2 After continuous OER catalysis for 10 h at the current density, the catalytic reaction potential did not change significantly, proving that the catalyst prepared in Example 1 has excellent OER electrocatalytic activity and stability.

[0146] The following is a charge-discharge cycle stability test of the catalyst prepared in Example 1 used as a cathode catalyst in a liquid zinc-air battery / flexible zinc-air battery / button-type zinc-air battery.

[0147] The catalyst prepared in Example 1 and the commercial Pt / C catalyst in Comparative Example 4 were assembled to obtain the cycle stability curves of two liquid zinc-air batteries at a current of 10 mA, as shown in the attached figures. Fig.15 and attached Fig.16 As shown, the liquid zinc-air battery assembled in Example 1 has a charge-discharge cycle stability of up to 1200 h, while the liquid zinc-air battery assembled with a commercial Pt / C catalyst has a charge-discharge cycle stability of only about 120 h. Therefore, the catalyst prepared in Example 1 is far superior to the commercial Pt / C catalyst corresponding to Comparative Example 4.

[0148] As attached Fig.17 As shown, under the condition of constant current of 1 mA, the liquid zinc-air battery assembled with the catalyst prepared in Example 1 has a charge-discharge cycle stability of more than 5200 h (30,000 cycles).

[0149] By the attached Fig.18As shown, after the catalyst prepared in Example 1 is assembled into a flexible zinc-air battery, the battery has good flexibility; under a constant current of 1 mA, the above-mentioned flexible zinc-air battery is subjected to a charge and discharge cycle stability test. The test found that during the bending / stretching process of the battery, the battery still has good charge and discharge cycle stability (more than 4200 min), indicating that the flexible zinc-air battery assembled with the catalyst prepared in Example 1 has good mechanical flexibility and long-term charge and discharge stability.

[0150] As attached Fig.19 As shown, under the condition of constant current of 1 mA, the button-type zinc-air battery assembled with the catalyst prepared in Example 1 has a charge-discharge cycle stability of more than 1000 min.

[0151] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0152] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a copper-based bimetallic single-atom catalyst, It is characterized in that include: (1-1) mixing the copper-based bimetallic precursor and the solvent to obtain a copper-based bimetallic precursor mixed solution; (1-2) mixing the copper-based bimetallic precursor mixed solution and the carrier carbon precursor to obtain the copper-based bimetallic single atom catalyst precursor solution; (2) extruding the copper-based bimetallic catalyst precursor solution to obtain a copper-based bimetallic single-atom catalyst precursor; (3) drying the copper-based bimetallic single atom catalyst precursor before pre-oxidation treatment, and pre-oxidizing the copper-based bimetallic single atom catalyst precursor; (4) calcining the pre-oxidized copper-based bimetallic single-atom catalyst precursor under an inert atmosphere to obtain a copper-based bimetallic single-atom catalyst; Wherein, in step (2), the extrusion treatment method includes at least one of solution air spinning, electrospinning and 3D printing, and / or the shape of the copper-based bimetallic single-atom catalyst precursor obtained by the extrusion treatment includes at least one of fiber, tubular and bamboo-shaped; The copper-based bimetallic precursor is a mixture of sodium copper chlorophyllin or copper phthalocyanine complex and sodium chloride; and / or, the carrier carbon precursor includes at least one of polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polystyrene and polyamide; and / or, the solvent includes at least one of N,N-dimethylformamide, dimethyl sulfoxide, cyclopentane sulfone and ethylene nitrate; The mass ratio of the copper-based bimetallic precursor to the carrier carbon precursor is (5-30):100; and / or the mass ratio of the solvent to the carrier carbon precursor is (5-12):1; In step (3), the pre-oxidation temperature is 200-280° C.; and / or the pre-oxidation time is 0.5-3 h; In step (4), the calcination temperature is 500-950° C.; and / or the calcination time is 1-3 hours.

2. The method according to claim 1, It is characterized in that In step (2), the extrusion treatment method is solution air spinning; And / or, the copper-based bimetallic single-atom catalyst precursor obtained by the extrusion process is in a fibrous shape.

3. The method according to claim 1, It is characterized in that The carrier carbon precursor is polyacrylonitrile; and / or the solvent is N,N-dimethylformamide.

4. The method according to claim 1, It is characterized in that The mass ratio of the copper-based bimetallic precursor to the carrier carbon precursor is (15-20):100; And / or, the mass ratio of the solvent to the carrier carbon precursor is (9-12):

1.

5. The method according to claim 1, It is characterized in that In step (3), the pre-oxidation temperature is 220-260°C; And / or, the pre-oxidation time is 2 to 3 h.

6. The method according to claim 1, It is characterized in that In step (4), the calcination temperature is 800-900°C; And / or, the calcination time is 1.5~2h.

7. A copper-based bimetallic single-atom catalyst, It is characterized in that The copper-based bimetallic single-atom catalyst is prepared by the method described in any one of claims 1-6.

8. A zinc-air battery, It is characterized in that A copper-based bimetallic single-atom catalyst prepared by the method according to any one of claims 1 to 6 or a copper-based bimetallic single-atom catalyst according to claim 7.

Citation Information

Patent Citations

  • Carbon-supported bimetallic monoatomic electrocatalyst, preparation method thereof, and application thereof

    CN110247061A

  • Bimetallic-activity monatomic catalyst for metal-air battery and preparation method thereof and metal-air battery

    CN110661008A