Monolithic catalyst and preparation method and application thereof
Through the integrated catalyst, combining precious metals and non-precious metal oxides, the problems of poor activity and high cost of catalytic combustion catalysts are solved, and catalytic combustion of volatile organic compounds such as cyclohexane with high efficiency and low energy consumption is achieved. It is suitable for cyclohexane-containing Organic exhaust gas treatment.
Patent Information
- Application Number
- CN202111220255.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-10-20
AI Technical Summary
The existing catalytic combustion catalysts have poor activity and are costly when treating organic waste gas containing cyclohexane. The combustion method has problems of high energy consumption and secondary pollution in the treatment of low-concentration VOCs.
Using a monolithic catalyst, including a honeycomb ceramic coated with alumina coating, supported by precious metals (platinum and palladium) and non-precious metal oxides (cobalt, iron, nickel, indium, etc.), it is prepared by impregnation treatment and calcination steps. Reduce the amount of precious metals and improve catalyst activity.
High conversion rate and selective catalytic combustion of volatile organic compounds such as cyclohexane under 200-450°C are achieved, energy consumption and operating costs are reduced, secondary pollution is avoided, and the catalyst activity is high and stable.
Smart Images

Figure BDA0003312331680000051 
Figure BDA0003312331680000061 
Figure BDA0003312331680000062
Abstract
Description
Technical Field
[0001] The invention relates to an integral catalyst and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds (VOCs) are highly volatile, easy to escape, and flammable and explosive. They are a type of air pollutant that seriously endangers human health and pollutes the environment. They mainly come from industries such as petrochemicals, pharmaceuticals, printing, painting, motor vehicles, and shoemaking. VOCs mainly include alkanes, alkenes, aromatics, halogenated hydrocarbons, ketones, acids, esters, and other compounds. Most volatile organic compounds have odors, cause pathological changes to the human body, and are even carcinogenic; especially volatile organic waste gases containing halogens, in addition to being highly toxic themselves, can also react photochemically with ozone to produce photochemical smog, which greatly damages the earth's environment. Therefore, controlling VOCs pollution has become an important task in the prevention and control of air pollution.
[0003] The treatment technology for volatile organic compounds is generally divided into two categories: recovery technology and degradation technology. Recovery technology includes adsorption, absorption, condensation, and membrane separation; degradation technology includes biodegradation, corona, photocatalysis, plasma treatment technology, combustion, etc. For high concentrations, recovery technology is directly used for recycling; for medium or low concentrations of VOCs, it is a better treatment method to use certain technologies to degrade them. Which technology to use depends on the specific situation, including the concentration, nature, and gas flow rate of the pollutants. The combustion method has certain advantages in treating low-concentration VOCs, and can be divided into direct flame combustion and catalytic combustion. The direct combustion method is to crack the harmful substances in the tail gas through high temperature, and the temperature of thermal cracking is as high as 800-900℃. This method requires a large amount of fuel oil, high operating costs, high energy consumption, low removal rate of halogen-containing organic matter, and will also produce nitrogen oxides. The catalytic combustion method uses the action of the catalyst to reduce the operating temperature to 280-450 degrees, greatly reducing energy consumption, safe and stable operation, reducing operating costs, and no nitrogen oxides, thereby no secondary pollution.
[0004] The catalysts used for catalytic combustion mainly include precious metal catalysts and non-precious metal catalysts. Due to their excellent ability to activate H2, O2, CH and OH bonds, precious metal element metals show very high activity in the oxidation reactions of hydrocarbons, H2 and CO. Therefore, precious metal catalysts show good activity in catalytic combustion reactions. Non-precious metal catalysts are generally transition metal oxide catalysts, single metal oxide catalysts, such as copper, manganese, cobalt and other metal oxides. These catalysts have low costs but average activity; there are also composite oxide catalysts. This type of catalyst is generally more active than the corresponding single oxide catalyst. For example, patent CN103252242B discloses a catalytic combustion catalyst of a composite oxide of copper, manganese and cerium. Summary of the invention
[0005] The present invention organically combines precious metals and non-precious metals to prepare an integral catalyst, which can reduce the amount of precious metals used and the cost of the catalyst, and has broad application prospects, such as being applied to the treatment of waste gas from a cyclohexanone device by a catalytic combustion method.
[0006] One of the technical problems to be solved by the present invention is that the catalyst for catalytic combustion of organic waste gas containing cyclohexane in the prior art has poor activity, and a new integral catalyst is provided. The prepared catalyst has the characteristics of high activity and good stability. The second technical problem solved by the present invention is a method for preparing the catalyst corresponding to the first technical problem. The third technical problem solved by the present invention is the application of the catalyst corresponding to the first technical problem in the treatment of organic waste gas containing cyclohexane.
[0007] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows:
[0008] A monolithic catalyst comprises a carrier and an active component, wherein the carrier is a honeycomb ceramic coated with an alumina coating, and the active component comprises 1) a noble metal, wherein the noble metal comprises platinum and palladium; and 2) a non-noble metal oxide, wherein the non-noble metal oxide comprises at least one of cobalt oxide, iron oxide, nickel oxide, indium oxide and niobium oxide.
[0009] According to some embodiments of the present invention, the content of the non-noble metal oxide loaded on the honeycomb ceramic per unit volume is 3-15 g / L.
[0010] According to some embodiments of the present invention, the aluminum oxide coating accounts for 4 to 21% of the total mass of the honeycomb ceramic, preferably 8 to 15%.
[0011] According to some embodiments of the present invention, the content of precious metals loaded on the honeycomb ceramic per unit volume is 150-1800 mg / L, specifically 200 mg / L, 400 mg / L, 500 mg / L, 700 mg / L, 800 mg / L, 1000 mg / L, 1200 mg / L, 1600 mg / L, 1700 mg / L, etc.
[0012] According to some embodiments of the present invention, the molar ratio of platinum to palladium in the precious metals loaded on the honeycomb ceramic per unit volume is (0.01-10):1, specifically 0.1:1, 0.25:1, 0.5:1, 0.8:1, 1.0:1, 1.5:1, 2.0:1, 2.5:1, 3.0:1, 5.0:1, etc.
[0013] To solve the second of the above technical problems, the technical solution adopted by the present invention is as follows:
[0014] A method for preparing a monolithic catalyst comprises the following steps: A) impregnating a honeycomb ceramic coated with an alumina coating with an alkaline solution, followed by drying and calcining; B) impregnating the calcined honeycomb ceramic with a noble metal salt solution and a non-noble metal salt solution, followed by drying and calcining to obtain a monolithic catalyst. In step A), the alkaline solution can regulate the pores in the alumina coating, thereby increasing the catalyst activity and reducing the reactor inlet temperature.
[0015] According to some embodiments of the present invention, the alkaline solution is an alkali metal hydroxide solution, preferably a sodium hydroxide solution. According to some embodiments of the present invention, in step A), the mass concentration of the alkali metal hydroxide solution is 0.5-6%.
[0016] According to some embodiments of the present invention, in step A), the immersion temperature is 20-40°C.
[0017] According to some embodiments of the present invention, in step A), the immersion time is 1 to 3 hours.
[0018] According to some embodiments of the present invention, in step A), the drying temperature is 100 to 120° C., and the drying time is 2 to 8 hours.
[0019] According to some embodiments of the present invention, in step A), the calcination temperature is 450-650° C., and the calcination time is 3-13 hours.
[0020] According to some embodiments of the present invention, in step B), the immersion temperature is 20-40°C.
[0021] According to some embodiments of the present invention, in step B), the drying temperature is 90 to 120° C., and the drying time can be 1 to 25 hours.
[0022] According to some embodiments of the present invention, in step B), the calcination temperature is 500-700° C., and the calcination time can be 3-13 hours.
[0023] According to some embodiments of the present invention, the preparation method further comprises the step a) preparing an aluminum-containing coating liquid by mixing pseudo-boehmite or alumina with urea, nitric acid and water, and then coating the aluminum-containing coating liquid on the honeycomb ceramic to obtain the honeycomb ceramic coated with the alumina coating.
[0024] According to some embodiments of the present invention, the preparation method of the aluminum-containing coating liquid comprises mixing pseudo-boehmite or alumina, urea, nitric acid and water to form an aluminum-containing slurry, stirring for 0.5 to 5 hours, and rubber grinding for 0.5 to 5 hours. According to some embodiments of the present invention, the mass ratio of pseudo-boehmite or alumina to water in the aluminum-containing slurry can be 0.05 to 0.8:1, the mass ratio of pseudo-boehmite or alumina to urea can be 1:0.3 to 2.5, and the mass ratio of pseudo-boehmite or alumina to concentrated nitric acid can be 1:0.01 to 0.2.
[0025] According to some embodiments of the present invention, when the aluminum-containing coating liquid is coated on the honeycomb ceramic, the drying temperature can be 100-125° C., the drying time can be 1-25 hours, the calcining temperature can be 300-600° C., and the calcining time can be 3-10 hours.
[0026] According to some embodiments of the present invention, the noble metal salt is selected from soluble acids or salts of platinum and palladium. According to some embodiments of the present invention, the non-noble metal salt is selected from nitrates, acetates or oxalates of cobalt salts and / or nickel salts and / or indium salts and / or niobium.
[0027] To solve the third technical problem, the technical solution adopted by the present invention is as follows: a method for purifying organic waste gas containing cyclohexane, comprising contacting the organic waste gas containing cyclohexane with the catalyst of the present invention, and introducing a mixture of nitrogen and oxygen or air at 200-450° C. Through the treatment method of the present invention, volatile organic matter such as cyclohexane can be catalytically burned to generate carbon dioxide and water.
[0028] The catalyst prepared by the present invention has high activity and can effectively reduce the concentration of cyclohexane in organic waste gas containing cyclohexane to 5000 mg / m 3 , benzene concentration 100mg / m 3 , toluene concentration 350mg / m 3 , airspeed 15000h -1Under the condition that when the catalyst bed inlet temperature is above 330°C, the conversion rate of each substance is above 99%, and the selectivity of the final product carbon dioxide is above 99%. The catalyst can be widely used in the catalytic oxidation combustion reaction of organic waste gas containing cyclohexane. DETAILED DESCRIPTION
[0029] The present invention will be further described below by way of examples.
[0030] Unless otherwise specified, the immersion temperature in the examples and comparative examples was carried out at room temperature (about 25-30° C.).
[0031] [Example 1-18]
[0032] 50g of alumina, 28g of urea, 5g of concentrated nitric acid and 100g of water were mixed and stirred for 40 minutes, then rubber-milled for 30 minutes to obtain alumina slurry, and then the honeycomb ceramic was immersed in the alumina slurry for 30 minutes, the honeycomb ceramic was taken out, and the residual liquid in the honeycomb ceramic was blown out with high-pressure nitrogen, and placed at room temperature for 8 hours, and heated from 20°C to 110°C at a heating rate of 0.5°C / min for 10 hours to dry, and then heated from 110°C to 550°C at a heating rate of 0.5°C / min for 6 hours to obtain a honeycomb ceramic coated with alumina coating. After multiple coatings, the proportion of alumina coating to the mass of honeycomb ceramic is shown in Table 1.
[0033] The obtained ceramic honeycomb coated with alumina coating was immersed in a sodium hydroxide aqueous solution at 30°C for a period of time (sodium hydroxide concentration and immersion time are shown in Table 1), then dried at 110°C for 4 hours and calcined at 550°C for 6 hours to obtain a ceramic honeycomb carrier.
[0034] Cobalt nitrate hexahydrate / or iron nitrate hexahydrate / or nickel nitrate hexahydrate / or indium nitrate / or niobium oxalate hexahydrate, chloroplatinic acid and palladium chloride were prepared into an aqueous solution according to the amounts given in Table 1, and then impregnated onto the honeycomb carrier. Then, the solution was dried at 110°C for 6 hours and calcined at 550°C for 6 hours to obtain a monolithic honeycomb catalyst.
[0035] Volume space velocity 15000h -1 , organic waste gas contains 5000mg / m 3 Cyclohexane, 100 mg / m 3 Benzene, 350mg / m 3 In the case of toluene, a catalytic combustion reaction occurs under the catalysis of the above-mentioned catalyst, and the reaction results are shown in Table 1.
[0036] [Comparative Examples 1-3]
[0037] 50g of alumina, 28g of urea, 5g of concentrated nitric acid and 100g of water were mixed and stirred for 40 minutes, then rubber-milled for 30 minutes to obtain alumina slurry, and then the honeycomb ceramic was immersed in the alumina slurry for 30 minutes, the honeycomb ceramic was taken out, and the residual liquid in the honeycomb ceramic was blown out with high-pressure nitrogen, and placed at room temperature for 8 hours, and heated from 20°C to 110°C at a heating rate of 0.5°C / min for 10 hours to dry, and then heated from 110°C to 550°C at a heating rate of 0.5°C / min for 6 hours to obtain a honeycomb ceramic coated with alumina coating. Through multiple coatings, the proportion of alumina coating to the mass of honeycomb ceramic is shown in Table 2.
[0038] Cobalt nitrate hexahydrate, chloroplatinic acid and palladium chloride were prepared into aqueous solution according to the amounts given in Table 2, and then impregnated into the honeycomb carrier, and then dried at 110°C for 6 hours and calcined at 550°C for 6 hours to obtain a monolithic honeycomb catalyst.
[0039] Volume space velocity 15000h -1 , organic waste gas contains 5000mg / m 3 Cyclohexane, 100mg / m 3 Benzene, 350mg / m 3 In the case of toluene, a catalytic combustion reaction occurs under the catalysis of the above-mentioned catalyst, and the reaction results are shown in Table 2.
[0040] Table 1
[0041]
[0042]
[0043] Table 2
[0044]
[0045] In Table 1 and Table 2, T1: the minimum inlet temperature when the cyclohexane conversion rate is above 99%, T2: the minimum inlet temperature when the benzene conversion rate is above 99%, and T3: the minimum inlet temperature when the toluene conversion rate is above 99%.
[0046] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A monolithic catalyst comprising a carrier and an active component, wherein: The carrier is a honeycomb ceramic coated with an alumina coating. The active components include 1) a noble metal, including platinum and palladium; and 2) a non-noble metal oxide, including cobalt oxide, The content of non-noble metal oxides loaded on the honeycomb ceramic per unit volume ranges from 7 to 15 g / L.
2. The monolithic catalyst according to claim 1, characterized in that The content of precious metals loaded on the honeycomb ceramic per unit volume is 150-1800 mg / L, wherein the molar ratio of platinum to palladium is (0.01-10):
1.
3. The monolithic catalyst according to any one of claims 1 to 2, characterized in that The aluminum oxide coating accounts for 4-21% of the total mass of the honeycomb ceramic.
4. The monolithic catalyst according to any one of claims 1 to 2, characterized in that The aluminum oxide coating accounts for 8-15% of the total mass of the honeycomb ceramic.
5. A method for preparing the monolithic catalyst according to any one of claims 1 to 4, comprising the following steps: A) impregnating the honeycomb ceramic coated with an alumina coating with an alkaline solution, and then drying and calcining; B) The honeycomb ceramic calcined in step A) is impregnated with a noble metal salt solution and a non-noble metal salt solution, and then dried and calcined to obtain a monolithic catalyst.
6. The preparation method according to claim 5, characterized in that: The alkaline solution is an alkali metal hydroxide solution.
7. The preparation method according to claim 6, characterized in that: In step A), the mass concentration of the alkali metal hydroxide solution is 0.5-6%; and / or the impregnation temperature is 20-40° C.; and / or the drying temperature is 100-120° C.; and / or the calcination temperature is 450-650° C.; and / or In step B), the drying temperature is 90-120°C, and / or the calcination temperature is 500-700°C.
8. The preparation method according to claim 7, characterized in that: In step A), the impregnation time is 1 to 3 hours; and / or the drying time is 2 to 8 hours; and / or the calcination time is 3 to 13 hours.
9. The preparation method according to any one of claims 5 to 8, characterized in that: The method also includes step a) preparing an aluminum-containing coating liquid by mixing pseudo-boehmite or alumina with urea, nitric acid and water, and then coating the aluminum-containing coating liquid on the honeycomb ceramic to obtain the honeycomb ceramic coated with the alumina coating.
10. The preparation method according to claim 9, characterized in that: The preparation method of the aluminum-containing coating liquid comprises the following steps: mixing pseudo-boehmite or alumina, urea, nitric acid and water to prepare an aluminum-containing slurry, stirring for 0.5 to 5 hours, and rubber grinding for 0.5 to 5 hours.
11. The preparation method according to claim 10, characterized in that: The mass ratio of pseudo-boehmite or alumina to water in the aluminum-containing slurry is 0.05-0.8:1, and / or the mass ratio of pseudo-boehmite or alumina to urea is 1:0.3-2.5, and / or the mass ratio of pseudo-boehmite or alumina to nitric acid is 1:0.01-0.
2.
12. The preparation method according to claim 9, characterized in that: When the aluminum-containing coating liquid is coated on the honeycomb ceramic, the drying temperature is 100-125° C. and the drying time is 1-25 hours; and / or the calcining temperature is 300-600° C. and the calcining time is 3-10 hours.
13. A method for purifying cyclohexane-containing organic waste gas, comprising contacting the cyclohexane-containing organic waste gas with the monolithic catalyst described in any one of claims 1 to 4 or the monolithic catalyst prepared by the preparation method described in any one of claims 5 to 12, and introducing a mixture of nitrogen and oxygen or air at 200 to 450°C.