A polypropylene composite film and its preparation method and application
By using a multi-layer structural film composed of homopolypolypropylene, propylene impact copolymer and polyolefin elastomer, the challenges of polypropylene film in impact resistance, optical properties and uniformity are solved, and efficient impact resistance and optical resistance are achieved. Performance combination.
Patent Information
- Application Number
- CN202111222002.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-20
AI Technical Summary
It is difficult for existing polypropylene films to have good impact resistance, optical properties and film uniformity at the same time, especially under high elastomer content, it is easy to lead to uneven film surface and uneven performance.
By adjusting the shear viscosity and components, using polypropylene composition A composed of homopolymer polypropylene, propylene impact copolymer and polyolefin elastomer. To form a multi-layer structural film, ensure uniformity of each layer and uniformity of performance.
The good impact resistance and optical properties of the polypropylene composite film are achieved, while ensuring the uniformity of the thickness and performance of the film in the MD and TD directions, improving the overall performance of the film.
Smart Images

Figure CN115991027B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of films, and in particular relates to a polypropylene composite film and a preparation method and application thereof. Background Art
[0002] Polypropylene film can usually be made by methods such as casting and biaxial stretching, but polypropylene film made from homopolymer polypropylene raw materials usually has low impact strength. Polypropylene film is often used for packaging purposes, which requires the film to have high impact performance. At the same time, for the visualization and aesthetics of the contents, the film is also expected to have good optical properties. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomers can be added to polypropylene, but the films prepared by the above methods usually have high haze and poor optical properties such as transparency. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.
[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method, such as CN101913279A, which uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3, and the elastomer provides good impact resistance, but this method has the problem of being difficult to disperse evenly when the elastomer content is high. And the elastomer usually has poor flow properties, which can cause uneven film surface, and the problem of large thickness difference along the machine direction (MD) and the transverse direction (TD). In the case of multi-layer co-extrusion, elastomer can also cause a large gap in the flow performance of the core surface layer, further aggravating the problem of uneven film surface, and may cause uneven performance of film everywhere. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good impact resistance, optical properties and film uniformity at the same time, and to provide a transparent impact-resistant polypropylene composite film with uniform thickness and properties at all parts of the film and a preparation method thereof. The polypropylene composite film has good impact resistance and optical properties at the same time, and has good film thickness and performance uniformity, with a thickness deviation in the MD direction of no more than 1.3, a thickness deviation in the TD direction of no more than 1.5, an impact performance deviation in the MD direction of no more than 0.05, and an impact performance deviation in the TD direction of no more than 0.07.
[0005] A first aspect of the present invention provides a polypropylene composite film, the polypropylene composite film comprising at least one film layer A formed of a polypropylene composition A and at least one film layer B formed of a polypropylene composition B; wherein the polypropylene composition A comprises homopolypropylene a, propylene impact copolymer b and polyolefin elastomer c, and the polypropylene composition B comprises random polypropylene x and polyolefin elastomer y;
[0006] The polyolefin elastomer c and the polyolefin elastomer y both meet the following conditions: at 230°C and a shear rate of 160r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.2-3, preferably 1.7-2.3, and at 230°C and a shear rate of 640r -1 Shear viscosity η 640 It is 100-500 Pa·s, preferably 140-400 Pa·s.
[0007] The second aspect of the present invention provides a method for preparing the polypropylene composite film, comprising: extruding and casting a raw material composition for forming each layer after an optional granulation process to form the composite film.
[0008] The third aspect of the present invention provides use of the polypropylene composite film in the field of packaging materials.
[0009] The composite film prepared by the present invention has good impact resistance and optical properties at the same time, and the film has good uniformity. The pendulum impact strength of the film of the present invention is ≥0.5J, and the film haze is ≤5%. In terms of uniformity, the thickness deviation in the MD direction is not greater than 1.3, the thickness deviation in the TD direction is not greater than 1.5, the impact performance deviation in the MD direction is not greater than 0.05, and the impact performance deviation in the TD direction is not greater than 0.07. Preferably, the pendulum impact strength of the film of the present invention is ≥1.1J, the film haze is ≤3%, the thickness deviation in the MD direction is not greater than 0.5, the thickness deviation in the TD direction is not greater than 0.75, the impact performance deviation in the MD direction is not greater than 0.03, and the impact performance deviation in the TD direction is not greater than 0.05.
[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Exemplary embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0012] Figure 1a and Figure 1b Schematic diagram of the film sampling point selection of the present invention.
[0013] Figure 2 This is an atomic force microscope photograph of a cross section of a thin film in one embodiment of the present invention. DETAILED DESCRIPTION
[0014] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0015] The present invention provides a polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises homopolypropylene a, propylene impact copolymer b and polyolefin elastomer c, and the polypropylene composition B comprises random polypropylene x and polyolefin elastomer y;
[0016] The polyolefin elastomer c and the polyolefin elastomer y both meet the following conditions: at 230°C and a shear rate of 160r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.2-3, preferably 1.7-2.3, and at 230°C and a shear rate of 640r -1 Shear viscosity η 640 It is 100-500 Pa·s, preferably 140-400 Pa·s.
[0017] According to the research conducted by the inventors, the thickness uniformity of a multilayer film is mainly affected by the uniformity of the film thickness within the layer. The rheological properties of the polyolefin elastomer are the main factors affecting the uniformity within each film layer. By adjusting the shear viscosity of the polyolefin elastomer to be within the scope of the present invention, the thickness uniformity and performance uniformity of the film can be greatly improved.
[0018] In addition, the thickness uniformity of the entire film is also affected by the fluidity matching degree of each layer of raw materials. Preferably, the polypropylene composition A and the polypropylene composition B are controlled at 230°C and a shear rate of 160r. -1 The difference in shear viscosity (ηA 160 -ηB 160 ) and at 230℃ and shear rate 640r -1 The difference in shear viscosity (ηA 640 -ηB 640 ) are both ≥ 0, and the ratio of the two (ηA 160 -ηB 160 ) / (ηA 640 -ηB 640 ) is 1-2.6, preferably 1.5-2.2. By adjusting the shear viscosity of the raw materials of different layers to be within the preferred range of the present invention, the uniformity of the film thickness and performance can be further improved.
[0019] According to some embodiments of the present invention, there are dispersed strip-shaped rubber phases in the composite film, the rubber phases are arranged parallel to each other, and the average width of the rubber phases is 20-200nm, and the average aspect ratio is 5-20. The "dispersed" mentioned herein means that the rubber phase is not continuously distributed in the composite film. The rubber phase can be seen by observing the cross section of the composite film cut along the transverse direction (TD) through an atomic force microscope (AFM), such as Figure 2 As shown in the black part, the rubber phase is in the form of multiple strips uniformly dispersed in the film matrix.
[0020] Herein, the "strip shape" refers to a shape whose aspect ratio is generally greater than 2.
[0021] The meaning of aspect ratio is well known to those skilled in the art. For strip particle testing, aspect ratio has the same concept as length-to-width ratio, that is, the ratio of the longest diameter passing through the inside of the particle to the longest diameter perpendicular to it. The former also corresponds to the length of the particle, and the latter corresponds to the width of the particle.
[0022] The average width and average aspect ratio are measured by observing the cross section of the composite film cut along the transverse direction (TD) using an atomic force microscope. Based on 200 sample points, the average value of the horizontal axis dimension of the rubber phase is calculated as the average width, and the average value of the aspect ratio of the rubber phase is calculated as the average aspect ratio.
[0023] The machine direction (MD) refers to the machining direction. The transverse direction (TD) refers to the direction perpendicular to the machining direction.
[0024] In the composite film of the invention, the rubber phases are advantageously arranged parallel to each other.
[0025] Herein, the term "parallel arrangement" means that the transverse cross sections of the rubber phase are arranged parallel to each other along a certain direction. This excludes a small amount of rubber phase particles arranged in different directions in a local area due to the preparation process and inconsistent with the overall arrangement direction of the rubber phase particles in the entire composite film, as well as rubber phase particles that cannot be clearly observed due to the preparation process or AFM method.
[0026] Herein, "parallel arrangement" includes substantially parallel conditions. The angle between the transverse cross sections of the rubber phases is not greater than about 10 degrees, preferably less than about 5 degrees.
[0027] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: pendulum impact strength ≥ 0.5J, preferably pendulum impact strength ≥ 1.1J; film haze ≤ 5%, preferably haze ≤ 3%; MD direction thickness deviation is not greater than 1.3, preferably not greater than 0.5; TD direction thickness deviation is not greater than 1.5, preferably not greater than 0.75; MD direction impact performance deviation is not greater than 0.05, preferably not greater than 0.03; TD direction impact performance deviation is not greater than 0.07, preferably not greater than 0.05.
[0028] According to some embodiments of the present invention, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available. For example, homopolypropylene with a grade of PPH-FA03 of Qingdao Refining and Chemical, homopolypropylene with a grade of PPH-FA03 of Zhongyuan Petrochemical, and homopolypropylene with a grade of FC801 of Shanghai Petrochemical. Alternatively, it can be prepared by conventional methods in the art.
[0029] According to the present invention, the propylene impact copolymer b is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymerization part containing ethylene units, preferably selected from ethylene-propylene copolymerization part and ethylene-butene copolymerization part. The elastic part can be shown as a spherical or nearly spherical rubber phase in a scanning electron microscope photo of an impact strip of the propylene impact copolymer.
[0030] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.
[0031] Based on the total weight of the propylene impact copolymer b, the content of the copolymerized part containing ethylene units in the propylene impact copolymer is preferably 3-15wt%, more preferably 7-12wt%. 13 C NMR determination.
[0032] Based on the total weight of the propylene impact copolymer b, the ethylene content of the propylene impact copolymer b is preferably 1-12wt%. In the room temperature xylene solubles of the propylene impact copolymer, the ethylene unit content is preferably not more than 40wt%. The ethylene unit group [EEE] content is preferably not more than 20wt%, by 13 C NMR determination.
[0033] The propylene impact copolymer b preferably has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.
[0034] The propylene impact copolymer may have a block structure or include a propylene block copolymer.
[0035] Propylene impact copolymers meeting the above characteristics are commercially available, such as propylene impact copolymers with the brand name EP200K from Sinopec, propylene impact copolymers with the brand name M180R from Shanghai Petrochemical, and propylene impact copolymers with the brand name PPB-M02D from Maoming Petrochemical.
[0036] The propylene impact copolymer can also be prepared by a continuous polymerization process in the presence of a Ziegler-Natta catalyst with high stereoselectivity. The continuous polymerization process means that the preparation process includes at least two sequential steps, wherein the elastic part and the non-elastic part are each prepared in a separate step, and, except for the first step, the latter step is carried out in the presence of the polymer formed in the previous step and the catalyst used in the previous step.
[0037] According to some embodiments of the present invention, the polyolefin elastomer c and the polyolefin elastomer y may each independently be an elastomeric copolymer of ethylene and an alpha olefin. The alpha olefin is preferably C3-C 12 The alpha olefin is preferably selected from at least one of propylene, 1-butene, 1-hexene and 1-octene. The polyolefin elastomer meeting the above characteristics is commercially available. For example, polyolefin elastomer with the trade mark of Dow 8200, polyolefin elastomer with the trade mark of Dow 8411, polyolefin elastomer with the trade mark of Mitsui DF840, polyolefin elastomer with the trade mark of Exxon VM3980. Alternatively, it can be prepared by conventional methods in the art.
[0038] When polyolefin elastomer is used in the composite film, the elastic part of the propylene impact copolymer and the polyolefin elastomer form a dispersed rubber phase in the composite film, which is in the form of strips and arranged parallel to each other. The specific features are as described above and will not be repeated here.
[0039] The presence of the polyolefin elastomer can advantageously compensate for the possible uneven distribution of the rubber phase in the propylene impact copolymer, thereby improving the uniformity of the impact properties of the film at various locations.
[0040] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.
[0041] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.
[0042] Random polypropylene meeting the above characteristics is commercially available, such as Yanshan Petrochemical's F5006 random polypropylene, Shanghai Petrochemical's F500EPS random polypropylene, and Shanghai Petrochemical's F800EDF random polypropylene; or can be prepared by conventional methods in the art.
[0043] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 40-90 wt% of homopolypropylene a, 5-40 wt% of propylene impact copolymer b and 2-30 wt% of polyolefin elastomer c.
[0044] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 55-75 wt% homopolypropylene a, 10-30 wt% propylene impact copolymer b and 5-20 wt% polyolefin elastomer c.
[0045] Since homopolypropylene contains relatively large spherulites, propylene impact copolymer and polyolefin elastomer contain rubber phases of different sizes, the refractive index of each component is different, and a synergistic effect will occur. According to the research of the inventors, the morphology and size of the rubber phase in the composition provided by the present invention can meet the requirements of the refractive index and obtain a film with good optical properties, and can also better absorb impact energy and meet the requirements of impact performance, so that the film has both good impact performance and optical properties.
[0046] According to some embodiments of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-95 wt% of the random polypropylene x and 5-60 wt% of the polyolefin elastomer y.
[0047] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 75-90 wt% of the random polypropylene x and 10-25 wt% of the polyolefin elastomer y.
[0048] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 2-7 g / 10 min.
[0049] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min.
[0050] When the melt mass flow rates of the polypropylene composition A and the polypropylene composition B are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity, mechanical properties and optical properties.
[0051] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A or the film layer B, or may have different compositions from the film layer A or the film layer B, or may be a mixture of a polypropylene composition A and a polypropylene composition B. When the polypropylene composite film has a structure of three or more layers, the film layer A is preferably used as an intermediate layer, such as a three-layer film including a film layer A, a film layer B, and a film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.
[0052] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:6-2:1, for example, it can be 1:5.5, 1:5, 1:4.5, 1:4, 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1 and any value therebetween.
[0053] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:4-1:1. Under this ratio, the composite film has good mechanical properties.
[0054] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.
[0055] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.
[0056] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.
[0057] According to the present invention, in order to improve other properties of the composite film (such as stability, antistatic property, etc.), the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-adhesive agent (anti-adhesive agent) and an antistatic agent. The specific type of the film-forming aid can be a conventional choice in the art, and the present invention is not particularly limited thereto.
[0058] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.
[0059] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0060] According to the present invention, before the extrusion process, the elastic part in the propylene impact copolymer used in the polymer composition as the raw material forms a rubber phase, which is spherical or nearly spherical and has an average particle size preferably less than or equal to 1.5 μm, and a maximum particle size preferably not more than 2 μm, as determined by observing the cross section of the specimen by SEM.
[0061] In the present invention, the spherical and nearly spherical particles refer to particles whose aspect ratios are substantially in the range of 1 to 2. “Substantially” means that at least 90% of the rubber phase particles have aspect ratios in the range of 1 to 2.
[0062] The average particle size and maximum particle size of the rubber phase in the propylene impact copolymer in the raw material are determined by observing the cross section of the impact spline by the scanning electron microscope (SEM) method, and the impact spline is prepared according to the method specified in the standard GB / T8809-2015. For spherical particles, the diameter of the particle is measured; for nearly spherical particles, the longitudinal axis of the particle (the distance between the two points on the particle contour that are farthest apart) is measured. The average value of the above dimensions of 50 sample points is obtained by SEM photo observation as the average particle size, and the maximum value of the above dimensions in the above sample points is taken as the maximum particle size.
[0063] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.
[0064] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.
[0065] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.
[0066] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.
[0067] By using the preparation method according to the present invention, the rubber phase contained in the propylene impact copolymer as the raw material is deformed during the preparation process of the composite film, changing from a spherical or nearly spherical shape to a strip shape, and is oriented in a certain direction, i.e. arranged in parallel, and such a microstructure is maintained in the final composite film product, thereby obtaining a composite film according to the present invention with good impact resistance and optical properties.
[0068] Advantageously, the polyolefin elastomer used also deforms during the preparation of the composite film, becoming a strip-shaped rubber phase and oriented in a certain direction, i.e. arranged in parallel, and such a microstructure is maintained in the final composite film product, while interacting synergistically with the rubber phase from the propylene impact copolymer, thereby further improving the impact resistance, optical properties and other properties of the composite film.
[0069] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as in the field of high-end packaging that requires both high impact resistance and optical properties of the film, including but not limited to battery packaging, electronic product packaging or food, especially high-end food packaging.
[0070] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0071] In the following examples and comparative examples:
[0072] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.
[0073] The polypropylene composition and film properties were tested according to the following methods:
[0074] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.
[0075] (2) Calculation of film pendulum impact strength and impact strength deviation: as shown in the attached Figure 1a As shown in the figure, after the film is trimmed, a point is taken every 1 meter along the MD direction on the center line of the film, and a total of 10 points are taken. The impact strength of each point is tested according to the method specified in GB / T 8809-2015, and the average value is taken as the impact strength of the film (MD). The standard deviation of the impact strength is calculated based on the above data as the impact strength deviation in the MD direction.
[0076] As attached Figure 1b As shown, 10 points are evenly selected along the TD direction of any part of the film, and the impact strength of each point is tested according to the method specified in GB / T8809-2015. The average value is the impact strength (TD) of the film. The standard deviation of the impact strength is calculated based on the above data as the impact strength deviation in the TD direction.
[0077] (4) Film haze: measured according to the method specified in GB / T 2410-2008.
[0078] (5) Film thickness and thickness deviation test: Use Japan Mitutoyo Model 7301 thickness gauge to test film thickness. Figure 1a As shown in the figure, after the film is trimmed, a point is taken every 1 meter along the MD direction on the center line of the film, and a total of 10 points are taken. The thickness of each point is tested according to the method specified in GB / T 8809-2015, and the average value is the thickness of the film (MD). The standard deviation of the thickness is calculated based on the above data as the thickness deviation in the MD direction.
[0079] As attached Figure 1b As shown, 10 points are evenly taken along the TD direction of any part of the film, and the thickness of each point is tested according to the method specified in GB / T8809-2015, and the average value is the thickness of the film (TD). The standard deviation of the thickness is calculated based on the above data as the thickness deviation in the TD direction.
[0080] (6) Calculation of standard deviation (S): Calculate according to formula (a).
[0081]
[0082] in, Represents the average value of the measured data X1, X2...Xn, and N is the total number of data used.
[0083] (7) Determination of shear viscosity. The shear viscosity was determined using a Rheograph 25 capillary rheometer from GOTTFERT, Germany, according to the method described in ISO11443:2014. The capillary rheometer temperature was set to 230°C, the die capillary length was 30 mm, the capillary aspect ratio was 30:1, and the preheating time was 300 seconds. The shear rate 160s -1 and 640s -1 The shear stress (δ) under the condition of , and the shear viscosity η under the corresponding shear rate are calculated according to formula (b) 160 and η 640 .
[0084]
[0085] The polypropylene composition A in the examples and comparative examples was subjected to a shear rate of 160 s -1 and 640s -1 The shear viscosity under 160 and ηA 640 , polypropylene composition B at a shear rate of 160s -1 and 640s -1 The shear viscosity under 160 and ηB 640 , P represents the shear rate of polypropylene composition A and polypropylene composition B at 160r -1 The difference in shear viscosity (ηA 160 -ηB 160 ) and 640r -1 The difference in shear viscosity (ηA 640 -ηB 640 ) ratio (ηA 160 -ηB 160 ) / (ηA 640 -ηB 640 ). ηA 160 , ηA 640 ,ηB 160 ,ηB 640 The specific values of and P are shown in Table 1.
[0086] The film properties in the examples and comparative examples are shown in Table 2.
[0087] (8) Atomic force microscopy (AFM) images: A Dimension FastScan Icon atomic force microscope (AFM) from Bruker Corporation of the United States was used to scan and observe the cross-section of the thin film sample along the transverse cut using the quantitative nanomechanical scanning mode.
[0088] (9) Method for determining the average width and average aspect ratio of the rubber phase of the film: Using the Dimension FastScan Icon atomic force microscope of Bruker Corporation of the United States, the quantitative nanomechanical scanning mode was used to scan and observe the cross section of the film sample, and the width of the rubber phase was measured and counted to obtain the average width (based on 200 sample points). The aspect ratio of the rubber phase is the ratio of its length direction to its width direction. After measurement, calculation and statistics, the average aspect ratio (based on 200 sample points) was obtained.
[0089] (10) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.
[0090] (11) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.
[0091] (12) The copolymer content containing ethylene units, ethylene unit content, and ethylene unit group [EEE] content in the propylene impact copolymer: 13 C NMR determination.
[0092] 13C NMR was measured using a 400MHz nuclear magnetic resonance spectrometer (NMR) from Bruker, Switzerland, model AVANCE III. The solvent was deuterated o-dichlorobenzene, 250mg sample / 2.5ml solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2mg of BHT antioxidant was added to the sample. The sample was dissolved at 140℃ and collected. 13 C-NMR, test temperature 125°C, probe head specification 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan times 6000 times.
[0093] Example 1
[0094] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0095] (1) Preparation of polypropylene composition A:
[0096] Component a is a homopolymer polypropylene with a brand name of PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is a propylene impact copolymer with a brand name of EP200K, purchased from China Petrochemical Corporation, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 13wt%, and a melt mass flow rate of 3.2g / 10min; component c is a polyolefin elastomer with a brand name of 8200, purchased from Dow, and is an ethylene-1-octene copolymer with an octene structural unit content of 38wt%. The polyolefin elastomer has a melt mass flow rate of 3.2g / 10min at 230°C and a shear rate of 160r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 2.18, and the elastomer is at 230°C and a shear rate of 640r -1 Shear viscosity η 640 is 185Pa·s. The components prepared above are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 75 parts by weight, the mass fraction Wb of component b is 10 parts by weight, and the mass fraction Wc of component c is 15 parts by weight. Then add a lubricant (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the sum of the masses of the above-mentioned components a, b and c is 100 parts by weight, and the amount of lubricant added is 0.1 parts by weight), and then add the mixture to a high-speed stirrer and mix evenly, and then add the mixed material to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. After the screw is melt-mixed, extruded, granulated and dried, polypropylene composition A pellets are obtained. The melt mass flow rate MFR is tested.A =3.8g / 10min.
[0097] (2) Preparation of polypropylene composition B:
[0098] Component x is a random polypropylene with a brand name of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer with a brand name of 8200, purchased from Dow, which is an ethylene-1-octene copolymer with an octene structural unit content of 38 wt%. The polyolefin elastomer has a melt flow rate of 5.2 g / 10 min at 230 ° C and a shear rate of 160 r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 2.18, and the elastomer is at 230°C and a shear rate of 640r -1 Shear viscosity η 640 The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 75 parts by weight, and the mass fraction Wy of component y is 25 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR is tested. B =4.2g / 10min.
[0099] (3) Preparation of composite films:
[0100] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.
[0101] The atomic force microscope photo of the cross section of the composite film is as follows Figure 2 As shown. The black part is the rubber phase, which is dispersed, strip-shaped, and arranged parallel to each other. The average width of the rubber phase is 84nm, and the average aspect ratio is 8.8.
[0102] Example 2
[0103] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0104] (1) Preparation of polypropylene composition A:
[0105] Component a is a homopolymer polypropylene with a brand name of PPH-FA03, purchased from Zhongyuan Petrochemical, with a melt mass flow rate of 3.0 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.6; component b is a propylene impact copolymer with a brand name of M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11 wt%, an ethylene-propylene copolymer content of 15 wt%, and a melt mass flow rate of 2.0 g / 10 min; component c is a polyolefin elastomer with a brand name of DF840, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 25 wt%. The polyolefin elastomer has a melt mass flow rate of 2.0 g / 10 min at 230°C and a shear rate of 160 r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.75, and the elastomer is at 230°C and a shear rate of 640r -1 Shear viscosity η 640 is 398Pa·s. The components prepared above are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 65 parts by weight, the mass fraction Wb of component b is 30 parts by weight, and the mass fraction Wc of component c is 5 parts by weight. Then add a lubricant (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the sum of the masses of the above-mentioned components a, b and c is 100 parts by weight, and the amount of lubricant added is 0.1 parts by weight), and then add the mixture to a high-speed stirrer and mix evenly, and then add the mixed material to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. After the screw is melt-mixed, extruded, granulated and dried, polypropylene composition A pellets are obtained. The melt mass flow rate MFR is tested. A =3.4g / 10min.
[0106] (2) Preparation of polypropylene composition B:
[0107] Component x is a random polypropylene with a brand name of F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3 g / 10 min; component y is a polyolefin elastomer with a brand name of DF840, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 25 wt%. The polyolefin elastomer has a shear rate of 160 r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.75, and the elastomer is at a shear rate of 640r-1 Shear viscosity η 640 The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 90 parts by weight, and the mass fraction Wy of component y is 10 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR is tested. B =5.6g / 10min.
[0108] (3) Preparation of composite films:
[0109] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide) is added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.
[0110] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 105 nm, and the average aspect ratio was 8.5.
[0111] Example 3
[0112] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0113] (1) Preparation of polypropylene composition A:
[0114] Component a is a homopolymer polypropylene with a brand name of FC801, purchased from Shanghai Petrochemical, with a melt mass flow rate of 7.8g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.8; component b is a propylene impact copolymer with a brand name of PPB-M02D, purchased from Maoming Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 10wt%, and an ethylene unit content of 36.3wt% and an ethylene unit group [EEE] content of 18.5wt% in its room temperature xylene solubles, and a melt mass flow rate of 1.5g / 10min; component c is a polyolefin elastomer with a brand name of VM3980, purchased from Exxon, a propylene-ethylene copolymer, an ethylene structural unit content of 9wt%, and the polyolefin elastomer has a melt mass flow rate of 1.5g / 10min at 230°C and a shear rate of 160r -1 and 640r -1The ratio of shear viscosity under 160 / η 640 is 2.26, and the elastomer is at 230°C and the shear rate is 640r -1 Shear viscosity η 640 is 205Pa·s. The components prepared above are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 55 parts by weight, the mass fraction Wb of component b is 25 parts by weight, and the mass fraction Wc of component c is 20 parts by weight. Then add a lubricant (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the sum of the masses of the above-mentioned components a, b and c is 100 parts by weight, and the amount of lubricant added is 0.1 parts by weight), and then add the mixture to a high-speed stirrer and mix evenly, and then add the mixed material to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230°C. After the screw is melt-mixed, extruded, granulated and dried, polypropylene composition A pellets are obtained. The melt mass flow rate MFR is tested. A =7.0g / 10min.
[0115] (2) Preparation of polypropylene composition B:
[0116] Component x is a random polypropylene with a grade of F800EDF, purchased from Shanghai Petrochemical, which is a propylene-ethylene binary copolymer with a melt mass flow rate of 7.8 g / 10 min; component y is a polyolefin elastomer with a grade of VM3980, purchased from Exxon, which is a propylene-ethylene copolymer with an ethylene structural unit content of 9 wt%. The polyolefin elastomer has a melt flow rate of 160 r / min at 230°C. -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 2.26, and the elastomer is at 230°C and the shear rate is 640r -1 Shear viscosity η 640 The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 80 parts by weight, and the mass fraction Wy of component y is 20 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR is tested. B =8.3g / 10min.
[0117] (3) Preparation of composite films:
[0118] The steps are the same as those in Example 2. The thickness of the film finally obtained is 50 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:4.
[0119] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, and mutually parallel rubber phases were observed. The average width of the rubber phase was 88 nm, and the average aspect ratio was 9.6.
[0120] Example 4
[0121] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0122] (1) Preparation of polypropylene composition A:
[0123] The steps are the same as those in Example 1, except that the mass fraction Wa of component a is 80 parts by weight, the mass fraction Wb of component b is 18 parts by weight, and the mass fraction Wc of component c is 2 parts by weight. Component c is a polyolefin elastomer with a grade of 8411, purchased from Dow, and is an ethylene-1-octene copolymer with an octene structural unit content of 36 wt%. The polyolefin elastomer is molten at 230°C and a shear rate of 160r. -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.80, and the elastomer is at 230°C and a shear rate of 640r -1 Shear viscosity η 640 The melt mass flow rate MFR of the obtained polypropylene composition A pellets was tested. A =2.6g / 10min.
[0124] (2) Preparation of polypropylene composition B:
[0125] The steps are the same as those in Example 1, except that the mass fraction Wx of component x is 92 parts by weight, and the mass fraction Wy of component y is 8 parts by weight. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR B =7.5g / 10min.
[0126] (3) Preparation of composite films:
[0127] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:6.
[0128] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 196 nm, and the average aspect ratio was 5.3.
[0129] Example 5
[0130] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0131] (1) Preparation of polypropylene composition A:
[0132] The steps are the same as those in Example 1, except that the mass fraction Wa of component a is 90 parts by weight, the mass fraction Wb of component b is 5 parts by weight, and the mass fraction Wc of component c is 5 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR A =3.0g / 10min.
[0133] (2) Preparation of polypropylene composition B:
[0134] The steps are the same as those in Example 1, except that the mass fraction Wx of component x is 80 parts by weight, and the mass fraction Wy of component y is 20 parts by weight. Finally, the polypropylene composition B pellets are obtained, and the melt mass flow rate MFR is tested. B =3.5g / 10min.
[0135] (3) Preparation of composite films:
[0136] The steps are the same as those in Example 2. The film thickness is 50 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 2:1.
[0137] Example 6
[0138] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0139] (1) Preparation of polypropylene composition A:
[0140] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 50 parts by weight, the mass fraction Wb of component b is 40 parts by weight, and the mass fraction Wc of component c is 10 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR A =4.8g / 10min.
[0141] (2) Preparation of polypropylene composition B:
[0142] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 60 parts by weight, and the mass fraction Wy of component y is 40 parts by weight. Finally, the polypropylene composition B pellets are obtained, and the melt mass flow rate MFR is tested. B =9.6g / 10min.
[0143] (3) Preparation of composite film: the steps are the same as those in Example 3.
[0144] When the composite film was observed under an atomic force microscope, dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 23 nm, and the average aspect ratio was 19.8.
[0145] Example 7
[0146] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0147] (1) Preparation of polypropylene composition A:
[0148] The steps are the same as those in Example 1, except that the mass fraction Wa of component a is 50 parts by weight, the mass fraction Wb of component b is 20 parts by weight, and the mass fraction Wc of component c is 30 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR A =2.0g / 10min.
[0149] (2) Preparation of polypropylene composition B:
[0150] The steps are the same as those in Example 1, except that the mass fraction Wx of component x is 85 parts by weight, and the mass fraction Wy of component y is 15 parts by weight. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR B =4.3g / 10min.
[0151] (3) Preparation of composite films:
[0152] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0153] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 145 nm, and the average aspect ratio was 12.1.
[0154] Example 8
[0155] A polypropylene film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 40 parts by weight, the mass fraction Wb of component b is 40 parts by weight, and the mass fraction Wc of component c is 20 parts by weight. The pellets of the polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.1g / 10min.
[0156] The composite film was observed under an atomic force microscope, and dispersed, strip-shaped, mutually parallel rubber phases were observed. The average width of the rubber phase was 88 nm, and the average aspect ratio was 17.0.
[0157] Example 9
[0158] A polypropylene film was prepared according to the method of Example 1, except that in the preparation of the polypropylene composition B, the mass fraction Wx of component x was 95 parts by weight, and the mass fraction Wy of component y was 5 parts by weight. Finally, pellets of the polypropylene composition B were obtained, and the melt mass flow rate MFR B =5.5g / 10min.
[0159] Example 10
[0160] A polypropylene film was prepared according to the method of Example 1, except that in the preparation of the polypropylene composition B, the mass fraction Wx of component x was 70 parts by weight, and the mass fraction Wy of component y was 30 parts by weight. Finally, pellets of the polypropylene composition B were obtained, and the melt mass flow rate MFR B =4.7g / 10min.
[0161] Embodiment 11
[0162] A polypropylene film was prepared according to the method of Example 1, except that in the preparation of the polypropylene composition B, the mass fraction Wx of component x was 40 parts by weight, and the mass fraction Wy of component y was 60 parts by weight. Finally, pellets of the polypropylene composition B were obtained, and the melt mass flow rate MFR B =3.2g / 10min.
[0163] Example 12
[0164] The polypropylene composition A was prepared according to the method of Example 3, and the polypropylene composition B was prepared according to the method of Example 2, so that (ηA 160 -ηB 160 ) and (ηA 640 -ηB 640 ) are all less than 0. A composite film was prepared according to the method of Example 3.
[0165] Comparative Example 1
[0166] The polypropylene film was prepared according to the method of Example 1, except that in the preparation process of the polypropylene composition A, the polyolefin elastomer C was replaced with a polyolefin elastomer with a grade of DF740 purchased from Mitsui Co., Ltd. The polyolefin elastomer was heated at 230°C and a shear rate of 160r. -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.63, and the elastomer is at 230°C and a shear rate of 640r -1 Shear viscosity η 640 The melt mass flow rate MFR of the polypropylene composition A was tested. A =2.4g / 10min.
[0167] Comparative Example 2
[0168] The polypropylene film was prepared according to the method of Example 2, except that in the preparation process of the polypropylene composition B, the polyolefin elastomer Y was replaced by a polyolefin elastomer with a grade of 8400 purchased from Dow Chemical Company. The polyolefin elastomer was heated at 230°C and a shear rate of 160r / min. -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 2.45, and the elastomer is at 230°C and the shear rate is 640r -1 Shear viscosity η 640 The melt mass flow rate MFR of the polypropylene composition B was tested. B =8.4g / 10min.
[0169] Comparative Example 3
[0170] A composite film was prepared according to the method of Example 1, except that the polypropylene composition B contained only component x.
[0171] Comparative Example 4
[0172] A composite film was prepared according to the method of Example 1, except that the polypropylene composition A contained only component a and component b, wherein the mass fraction Wa of component a was 75 parts by weight, and the mass fraction Wb of component b was 25 parts by weight.
[0173] Comparative Example 5
[0174] A composite film was prepared according to the method of Example 1, except that the polypropylene composition A contained only component a and component c, wherein the mass fraction Wa of component a was 75 parts by weight, and the mass fraction Wc of component c was 25 parts by weight.
[0175] Table 1
[0176]
[0177] Table 2
[0178]
[0179] It can be concluded from the results of the embodiments in Table 1 that the polypropylene composite film provided by the present invention has good impact resistance and optical properties at the same time, and has good film uniformity. The pendulum impact strength of the film of the present invention is ≥0.5J, and the film haze is ≤5%. In terms of uniformity, the thickness deviation in the MD direction is not greater than 1.3, the thickness deviation in the TD direction is not greater than 1.5, the impact performance deviation in the MD direction is not greater than 0.05, and the impact performance deviation in the TD direction is not greater than 0.07. It can be seen from the preferred embodiment that the pendulum impact strength of the film of the present invention is ≥1.1J, the film haze is ≤3%, the thickness deviation in the MD direction is not greater than 0.5, the thickness deviation in the TD direction is not greater than 0.75, the impact performance deviation in the MD direction is not greater than 0.03, and the impact performance deviation in the TD direction is not greater than 0.05. It can be seen from the comparative example that the use of polyolefin elastomers other than the present invention or the change in the proportion of the film layer components will lead to a decrease in film performance, and during extrusion casting, the film surface is unstable, and the uniformity of film thickness and impact performance is greatly reduced.
[0180] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0181] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene composite film, characterized in that: The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B; wherein the polypropylene composition A comprises homopolymerized polypropylene a, propylene impact copolymer b and polyolefin elastomer c, and the polypropylene composition B comprises random polypropylene x and polyolefin elastomer y; The polyolefin elastomer c and the polyolefin elastomer y both meet the following conditions: at 230°C and a shear rate of 160r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.2-3, and at 230°C and a shear rate of 640r -1 Shear viscosity η 640 100-500Pa·s; The polypropylene composite film contains dispersed strip-shaped rubber phases, which are arranged parallel to each other, and have an average width of 20-200 nm and an average aspect ratio of 5-20. Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 40-90 wt% of homopolypropylene a, 5-40 wt% of propylene impact copolymer b and 2-30 wt% of polyolefin elastomer c; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-95 wt% of random polypropylene x and 5-60 wt% of polyolefin elastomer y; The propylene impact copolymer b is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer b, the ethylene content of the propylene impact copolymer b is 1-12wt%; the polyolefin elastomer c and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and alpha olefin.
2. The polypropylene composite film according to claim 1, characterized in that: The polyolefin elastomer c and the polyolefin elastomer y both meet the following conditions: at 230°C and a shear rate of 160r -1 and 640r -1 The ratio of shear viscosity under 160 / η 640 is 1.7-2.3, and at 230°C and a shear rate of 640r -1 Shear viscosity η 640 It is 140-400Pa·s.
3. The polypropylene composite film according to claim 1, characterized in that: The angles between the transverse sections of the rubber phase are no greater than 10 degrees, which is determined by observing the cross section of the composite film cut along the transverse direction (TD) using an atomic force microscope.
4. The polypropylene composite film according to claim 3, characterized in that: The angles between the transverse cross sections of the rubber phase are less than 5 degrees.
5. The polypropylene composite film according to claim 1, characterized in that: The polypropylene composite film has at least one of the following characteristics: pendulum impact strength ≥ 0.5J; film haze ≤ 5%; MD direction thickness deviation is not greater than 1.3; TD direction thickness deviation is not greater than 1.5; MD direction impact performance deviation is not greater than 0.05; TD direction impact performance deviation is not greater than 0.
07.
6. The polypropylene composite film according to claim 5, characterized in that: The pendulum impact strength is ≥1.1J.
7. The polypropylene composite film according to claim 5, characterized in that: The haze is ≤3%.
8. The polypropylene composite film according to claim 5, characterized in that: The thickness deviation in the MD direction is not greater than 0.
5.
9. The polypropylene composite film according to claim 5, characterized in that: The thickness deviation in the TD direction is no more than 0.
75.
10. The polypropylene composite film according to claim 5, characterized in that: The impact performance deviation in the MD direction is no more than 0.
03.
11. The polypropylene composite film according to claim 5, characterized in that: The TD direction impact performance deviation is no more than 0.
05.
12. The polypropylene composite film according to claim 1, characterized in that: At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min.
13. The polypropylene composite film according to claim 12, characterized in that: At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-7 g / 10 min; At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 4-8 g / 10 min.
14. The polypropylene composite film according to claim 1, characterized in that: The polypropylene composition A and the polypropylene composition B were heated at 230°C and a shear rate of 160r -1 The difference in shear viscosity (ηA 160 -ηB 160 ) and at 230℃ and shear rate 640r -1 The difference in shear viscosity (ηA 640 -ηB 640 ) are both ≥ 0, and the ratio of the two (ηA 160 -ηB 160 ) / (ηA 640 -ηB 640 ) is 1-2.
6.
15. The polypropylene composite film according to claim 14, characterized in that: The polypropylene composition A and the polypropylene composition B were heated at 230°C and a shear rate of 160r -1 The difference in shear viscosity (ηA 160 -ηB 160 ) and at 230℃ and shear rate 640r -1 The difference in shear viscosity (ηA 640 -ηB 640 ) ratio (ηA 160 -ηB 160 ) / (ηA 640 -ηB 640 ) is 1.5-2.
2.
16. The polypropylene composite film according to claim 1, characterized in that: The homopolymer polypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.
0.
17. The polypropylene composite film according to claim 1, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer b has a content of 3-15wt%; In the room temperature xylene soluble matter of the propylene impact copolymer, the ethylene unit content is not more than 40wt%, the ethylene unit group EEE content is not more than 20wt%, and the 13 C NMR determination; The propylene impact copolymer b has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.
18. The polypropylene composite film according to claim 17, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer b has a content of 7-12 wt %.
19. The polypropylene composite film according to claim 1, characterized in that: The alpha olefin is C3-C 12 of alpha olefins.
20. The polypropylene composite film according to claim 19, characterized in that: The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
21. The polypropylene composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.
22. The polypropylene composite film according to claim 21, characterized in that: The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.
23. The polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 55-75 wt% of homopolypropylene a, 10-30 wt% of propylene impact copolymer b and 5-20 wt% of polyolefin elastomer c.
24. The polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 75-90 wt% of the random polypropylene x and 10-25 wt% of the polyolefin elastomer y.
25. The polypropylene composite film according to any one of claims 1 to 24, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:6-2:
1.
26. The polypropylene composite film according to claim 25, characterized in that: In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-1:
1.
27. The polypropylene composite film according to any one of claims 1 to 24, characterized in that: When the polypropylene composite film has a structure of three or more layers, the film layer A is the middle layer.
28. The polypropylene composite film according to any one of claims 1 to 24, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.
29. The polypropylene composite film according to claim 28, characterized in that: The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.
30. The polypropylene composite film according to claim 28, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.
31. The polypropylene composite film according to claim 30, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.2-0.4 parts by weight.
32. The polypropylene composite film according to claim 28, characterized in that: The lubricant is a PEG lubricant and / or a monoglyceride lubricant.
33. The polypropylene composite film according to claim 28, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.
34. The polypropylene composite film according to claim 33, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.
35. The polypropylene composite film according to any one of claims 1 to 24, characterized in that: The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.
36. The polypropylene composite film according to claim 35, characterized in that The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-sticking agent and an antistatic agent.
37. The polypropylene composite film according to claim 35, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.
38. The polypropylene composite film according to claim 37, characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.
39. The method for preparing the polypropylene composite film according to any one of claims 1 to 38, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.
40. The preparation method according to claim 39, characterized in that: The stretching is bidirectional stretching.
41. Use of the polypropylene composite film according to any one of claims 1 to 38 in the field of packaging materials.
42. The use according to claim 41, characterized in that The packaging is battery packaging, electronic product packaging or food packaging.