A catalyst for dehydrogenating six-membered cycloalkane to produce aromatics and preparation method thereof
By using alumina support containing sulfate and specific metal components, the catalyst is easily deposited and has low stability, the aromatic selectivity and activity stability of the six-membered cycloalkane dehydrogenation catalyst is improved, and the by-product ring is realized Effective utilization of hexane and efficient regeneration of catalysts.
Patent Information
- Application Number
- CN202111227609.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-21
AI Technical Summary
The existing six-membered cycloalkane dehydrogenation catalysts have problems such as catalysts that are prone to carbon accumulation, low stability and frequent regeneration, and it is difficult to effectively utilize the by-product cyclohexane, which affects the production efficiency and safety of cyclohexamide.
Alumina containing sulfate is used as a support to support Group VIII metals, Group VIIB metals, P and K to form alloys or new active centers, inhibit metal aggregation, improve the acidity and regeneration properties of the catalyst, and extend the catalyst life.
The aromatic hydrocarbon selectivity and activity stability are improved, the carbon deposit rate of the catalyst is reduced, the single-pass reaction life of the catalyst is extended, and the regeneration performance of the catalyst is improved, achieving the effective utilization of the by-product cyclohexane.
Smart Images

Figure BDA0003314732300000021 
Figure BDA0003314732300000031 
Figure BDA0003314732300000111
Abstract
Description
Technical Field
[0001] The present invention relates to a cycloalkane dehydrogenation catalyst and a preparation method thereof, in particular to a hexacycloalkane dehydrogenation catalyst for producing aromatic hydrocarbons and a preparation method thereof. Background Art
[0002] Six-membered cycloalkanes refer to cyclohexane and alkyl-substituted cyclohexanes, including cyclohexane, methylcyclohexane, ethylcyclohexane, 1,2-dimethylcyclohexane, 1,3-dimethylcyclohexane, and 1,4-dimethylcyclohexane. After dehydrogenation, they can generate corresponding benzene, toluene, ethylbenzene, and xylene. In addition, cycloalkanes have received extensive attention as organic liquid hydrogen storage materials. The dehydrogenation reaction of cycloalkanes is the main reaction for hydrogen production, and its core is the cycloalkanes dehydrogenation catalyst.
[0003] Cyclohexane is generally used as a solvent, a standard substance for chromatography analysis, and for organic synthesis. It can be used in resins, coatings, fats, paraffin oils, and can also be used to prepare organic substances such as benzene, cyclohexene, cyclohexanol, and cyclohexanone. The main production process of the caprolactam unit is to generate caprolactam through reactions such as hydrogenation of raw benzene, hydration of cyclohexene, dehydrogenation of cyclohexanol to generate cyclohexanone, ammoximation of cyclohexanone, and rearrangement of cyclohexanone oxime. In the process of hydration-based cyclohexanone production, cyclohexane as a byproduct is produced, so that the effective utilization rate of raw benzene can only reach about 75%. The utilization of byproduct cyclohexane has always been a major problem in the caprolactam industry. With little market demand, almost all companies sell it at a low price. The storage and transportation of large amounts of cyclohexane materials increase the safety risks and operating costs of companies. Under certain temperature, pressure and catalyst, the byproduct cyclohexane of the cyclohexanone unit is directly converted into benzene and hydrogen, and then the benzene and hydrogen are recycled back to the cyclohexanone unit as raw materials, so that the byproduct cyclohexane can be effectively utilized, and the closed-loop circulation of raw materials and products in the unit can be realized, achieving the purpose of green, environmental protection, high efficiency, energy saving and no waste generation, while reducing the purchase of raw material benzene and the load of the supporting hydrogen production unit. Therefore, greatly improving the high selectivity of cyclohexane into benzene can bring leapfrog progress to the caprolactam industry.
[0004] The dehydrogenation of hexacycloalkanes is a highly endothermic reaction. From the perspective of kinetics and thermodynamics, increasing the temperature and reducing the pressure are conducive to the dehydrogenation to produce aromatics. However, increasing the temperature also increases the occurrence of side reactions. Taking cyclohexane as an example, byproducts such as methylcyclopentane, cyclohexene, n-hexane, 2-methylpentane, and 3-methylpentane may also be generated. After reducing the pressure, the rate of catalyst carbon deposition is accelerated, which will affect the single-pass life of the catalyst and the catalyst needs to be regenerated frequently. Therefore, this puts higher requirements on the development of new hexacycloalkanes dehydrogenation catalysts.
[0005] CN1201715A discloses a saturated hydrocarbon dehydrogenation catalyst and a preparation method thereof, wherein a large-aperture double-pore-distributed γ-Al2O3 sphere is used as a carrier, and Pt, Sn and K are loaded to prepare a catalyst for C 10 ~C 14 Dehydrogenation reaction of straight-chain alkanes. USP6103103 discloses a method for producing olefins by dehydrogenating hydrocarbon raw materials, wherein the catalyst used has borosilicate molecular sieve as a carrier, platinum metal as an active metal, zinc as an auxiliary agent, and also contains alkaline earth metal. These catalysts generally have the problem of easy carbon deposition and deactivation of the catalyst and low catalyst stability.
[0006] CN107537560A discloses a dehydrogenation catalyst, which uses modified MCM-41 as a carrier and loaded with platinum to prepare a catalyst for dehydrogenation reaction of organic liquid hydrogen storage materials, wherein the organic liquid hydrogen storage materials are selected from methylcyclohexane, cyclohexane, tetralin, decalin, etc. However, the MCM-41 molecular sieve is a pure silicon molecular sieve, which has weak acidity. While inhibiting carbon deposition, the dispersion and activity of Pt metal do not have obvious advantages, and the traditional Al2O3 carrier has too strong acidity, resulting in serious carbon deposition on the catalyst surface.
[0007] CN104785256B discloses a method for preparing a catalyst for preparing cyclohexene by dehydrogenating cycloalkanes, wherein Mg-Al hydrotalcite containing at least one of tin, indium and gallium is calcined in a microwave field to prepare a Mg-Al-O composite oxide carrier containing a promoter, and then platinum is introduced by impregnation to prepare a catalyst, the purpose of which is to improve the anti-coking performance of the carrier. However, if the catalyst is used for the reaction of preparing cyclohexene by dehydrogenating cycloalkanes and the dehydrogenation activity is to be further improved to prepare benzene, it is still necessary to further improve the properties of the active metal and the carrier of the catalyst to improve the anti-coking performance of the catalyst.
[0008] CN110882703A discloses a cycloalkane dehydrogenation catalyst containing alkaline earth metal and a preparation method thereof, wherein Pt is used as an active metal component, Sn is used as an auxiliary component, and the carrier is an alumina carrier containing alkaline earth metal, sulfur and titanium. The catalyst is used for the dehydrogenation of cyclohexane to produce benzene, but has the problems of low cyclohexane conversion rate, low catalyst stability, high carbon deposition and frequent regeneration. Summary of the invention
[0009] The purpose of the present invention is to provide a catalyst for dehydrogenating hexacycloalkane to produce aromatics and a preparation method thereof. The catalyst is used for the dehydrogenation of hexacycloalkane to produce aromatics and has high aromatics selectivity, activity stability and good regeneration performance.
[0010] The catalyst for dehydrogenating hexacyclic alkane to aromatics provided by the present invention comprises an alumina carrier containing sulfate and components having the following contents calculated based on the alumina:
[0011]
[0012] The present invention uses sulfate-containing alumina as a carrier to load active components to prepare a catalyst. The catalyst has high aromatics selectivity, good activity stability and good regeneration performance under the operating conditions of high temperature, low pressure and low hydrogen / hydrocarbon volume ratio. DETAILED DESCRIPTION
[0013] The catalyst of the present invention uses alumina containing sulfate as a carrier, and loads active components of Group VIII metal, Group VIIB metal, P and K, so that the main active component Group VIII metal of the catalyst can play a better dehydrogenation function, and the Group VIIB metal can form an alloy or a new active center with the Group VIII metal to inhibit the agglomeration of Group VIII metal grains, especially Pt grains. The addition of K and P can improve the acidity of the catalyst, reduce the occurrence of hydrogenolysis and cracking side reactions, reduce the carbon deposition rate of the catalyst, extend the catalyst single-pass reaction life, and improve the regeneration performance of the catalyst. The sulfur in the alumina carrier containing sulfate can be released when the catalyst is reduced, so that the reduction is carried out while the sulfurization is carried out during the reduction process, and the catalyst does not need to be pre-sulfurized after reduction.
[0014] Preferably, the content of each component of the catalyst of the present invention is:
[0015]
[0016] In the catalyst of the present invention, the Group VIII metal is selected from platinum, ruthenium or rhodium, more preferably platinum, the Group VIIB metal is preferably rhenium, and the halogen is preferably chlorine.
[0017] The sulfate-containing alumina is preferably sulfate-containing γ-alumina.
[0018] Preferably, the sulfate-containing alumina described in the present invention has the following pore radius distribution: pores with a pore radius of 3 to 5 nm account for 45 to 58 volume % of the total pore volume, pores with a pore radius of 5 to 10 nm account for 41 to 50 volume % of the total pore volume, and pores with a pore radius greater than 10 nm account for 1 to 8 volume % of the total pore volume.
[0019] The sulfate-containing alumina described in the present invention more preferably has the following pore radius distribution: pores with a pore radius of 3 to 5 nm account for 45 to 55 volume % of the total pore volume, pores with a pore radius of 5 to 10 nm account for 41 to 48 volume % of the total pore volume, and pores with a pore radius greater than 10 nm account for 4 to 7 volume % of the total pore volume.
[0020] The specific surface area of the sulfate-containing aluminum oxide of the present invention is preferably 200 to 220 m 2 / g, and the pore volume is preferably 0.6 to 0.9 mL / g.
[0021] The sulfate-containing alumina carrier of the present invention may be in the shape of a sphere, a strip, a sheet, a particle or a cloverleaf, preferably a strip, a sphere or a cloverleaf.
[0022] There are two methods for preparing the catalyst described in the present invention. One is a co-impregnation method, that is, the impregnation liquid contains all active components, and all active components are introduced into the carrier by one-step impregnation. The other is a separate impregnation method, that is, phosphorus and potassium are first introduced into the carrier, and then the Group VIII metal and Group VIIB metal are introduced after drying and calcination.
[0023] Specifically, the method for preparing the catalyst by co-impregnation method comprises impregnating a sulfate-containing alumina carrier with a solution containing Group VIII metal compounds, Group VIIB metal compounds, phosphorus-containing compounds, potassium-containing compounds and halogen as an impregnation liquid, and drying and calcining the impregnated solid.
[0024] The method for preparing the catalyst by using a fractional impregnation method comprises:
[0025] (1) impregnating a sulfate-containing alumina carrier with a solution of a phosphorus-containing compound and a potassium-containing compound as an impregnation liquid, drying and calcining the alumina carrier;
[0026] (2) The carrier calcined in step (1) is impregnated with a solution containing a Group VIII metal compound, a Group VIIB metal compound and a halogen as an impregnation solution, and the impregnated solid is dried and calcined.
[0027] In the above preparation method, the Group VIII metal compound is preferably chloroplatinic acid, tetraammonium platinum dichloride, ammonium chloroplatinate, platinum trichloride, platinum tetrachloride hydrate, dicarbonyl platinum dichloride, dinitrodiaminoplatinum or sodium tetranitroplatinate; the Group VIIB metal compound is preferably perrhenic acid or ammonium perrhenate; the phosphorus-containing compound is preferably phosphoric acid, phosphorous acid or pyrophosphoric acid, the potassium-containing compound is preferably potassium chloride or potassium hydroxide, and the halogen is preferably chlorine.
[0028] In the above method, the method of introducing active components by impregnation can be saturated impregnation or supersaturated impregnation. During saturated impregnation, the liquid / solid volume ratio of the impregnation solution to the carrier is less than 1.0, preferably 0.5-0.9, and the impregnation solution is completely absorbed by the carrier. The liquid / solid volume ratio of the impregnation solution used for supersaturated impregnation to the carrier is greater than 1.0, preferably 1.1-3.0. After impregnation, the excess impregnation solution is removed by filtering or vacuum evaporation of the solvent. The vacuum evaporation method of the solvent can be carried out using a rotary vacuum evaporator. The specific operation method is: the water-soluble compound containing each active component is prepared into an impregnation solution, and the sulfate-containing aluminum oxide is impregnated under the conditions of 0.001-0.10MPa and rotation. The liquid / solid volume ratio of the impregnation solution to the sulfate-containing aluminum oxide is 1.1-3.0, and the rotation linear speed is 0.01-2.0 m / s. After impregnation, it is dried and calcined for activation. The pressure of vacuum rotary impregnation is preferably 0.001-0.08MPa. During the impregnation, the catalyst is heated and rotated at the same time. The heating temperature, i.e., the impregnation temperature, is preferably 20 to 60°C, more preferably 20 to 40°C. The rotation rate should not be too fast. The preferred rotation linear speed is 0.02 to 0.8 m / s, more preferably 0.03 to 0.5 m / s. The impregnation time is preferably 1 to 8 hours, more preferably 2 to 4 hours. After the vacuum rotary impregnation, the water in the impregnation liquid has been basically evaporated, and the catalyst is in a dry state. At this time, the carrier can be directly taken out for drying and calcination.
[0029] In the above method, both the co-impregnation method and the separate impregnation method (2) are steps for introducing Group VIII metals into the carrier. To facilitate the introduction of halogen components and the uniform distribution of Group VIII metals, especially platinum, on the entire carrier, the impregnation solution preferably contains a competitive adsorbent, which is selected from one or more of hydrochloric acid, trichloroacetic acid, citric acid, acrylic acid and methanol. The preferred competitive adsorbent is hydrochloric acid and / or citric acid. When the two are used simultaneously, they can be added to the impregnation solution separately or simultaneously. The mass ratio of HCl to citric acid in the impregnation solution is 0.01 to 50:1, preferably 0.2 to 10:1. The concentration of the competitive adsorbent in the impregnation solution is 0.2 to 3.0% by mass, preferably 0.8 to 2.0% by mass, calculated as chlorine. If citric acid is added to the impregnation solution as a competitive adsorbent, after the carrier is dried, it is preferably heated at 150 to 230°C for 0.5 to 24 hours to desorb the citric acid from the carrier.
[0030] In the above method, the drying temperature of the solid obtained after the active component is introduced by impregnation is preferably 110-150°C, and the drying time is preferably 6-24 hours; the calcination temperature is preferably 450-550°C, and the calcination time is preferably 2-8 hours.
[0031] The method for preparing the sulfate-containing alumina carrier of the present invention comprises the following steps:
[0032] (1) Mixing a sodium aluminate solution and an aluminum sulfate solution, controlling the pH value thereof to 8.5 to 9.2, reacting at 50 to 80° C. for 0.3 to 1 hour, then adding a sodium carbonate solution to adjust the pH value of the system to 9.5 to 9.8, continuing the reaction for 0.3 to 1 hour, then heating to 98 to 150° C. for aging for 1.5 to 8 hours, washing the obtained solid with water, and drying to obtain aluminum hydroxide powder containing sulfate groups,
[0033] (2) mixing the aluminum hydroxide powder containing sulfate with a peptizing agent, extruding into strips, drying, and calcining at 450-700° C. to obtain aluminum oxide containing sulfate.
[0034] (3) treating the sulfate-containing aluminum oxide with steam at 580-700° C. for 1-3 hours, wherein the gas / solid volume ratio is controlled to be 0.5-100:1 during the steam treatment, and the mass ratio of the steam to the sulfate-containing aluminum oxide is 1:80-300.
[0035] In the method for preparing the sulfate-containing alumina carrier, step (1) is to prepare the sulfate-containing aluminum hydroxide powder, wherein the concentration of the sodium aluminate solution used is preferably 150-300 g / L, the alumina content in the sodium aluminate solution is 60-70% by mass, the Na2O content is 30-40% by mass, the concentration of the aluminum sulfate solution is preferably 20-65 g / L, and the concentration of the sodium carbonate solution is preferably 10-30 g / L. The solid obtained after aging is preferably washed 5-20 times, the drying temperature is preferably 100-200° C., and the drying time is preferably 4-24 hours.
[0036] The method (2) is a carrier molding step, wherein the peptizing agent is an acid solution, wherein the acid is selected from one or more of hydrochloric acid, nitric acid, acetic acid and citric acid, and the concentration of the acid contained in the peptizing agent is preferably 2 to 13% by mass, more preferably 3 to 10% by mass, and the mass ratio of the peptizing agent to the peptized powder is preferably 0.5 to 0.8. The drying temperature in step (2) is preferably 100 to 200°C, and the time is preferably 4 to 24 hours. The calcination temperature is preferably 500 to 650°C, and the calcination time is preferably 2 to 6 hours.
[0037] The method (3) comprises treating the formed carrier in step (2) with steam to increase the macropore content. The steam treatment temperature is preferably 600-680°C, the water used for the steam treatment is preferably saturated steam at 100-150°C, the steam treatment time is preferably 1.5-3 hours, the gas / solid volume ratio controlled during the steam treatment is preferably 5-40:1, and the mass ratio of the steam used for the steam treatment to the sulfate-containing aluminum oxide is preferably 1:100-260.
[0038] The catalyst of the present invention needs to be reduced with hydrogen before use, the reduction temperature is preferably 450-520°C, the reduction time is preferably 2-6 hours, and the reduction gas / agent volume ratio is preferably 400-1500:1.
[0039] The catalyst of the present invention is suitable for the dehydrogenation reaction of six-membered cycloalkanes, wherein the six-membered cycloalkanes are cyclohexane and alkyl-substituted cyclohexane, wherein the substituted alkyl is a C1-C2 alkyl, and the number of the substituted alkyl can be multiple, preferably 1-2, such as cyclohexane, methylcyclohexane, ethylcyclohexane, 1,2-dimethylcyclohexane, 1,3-dimethylcyclohexane, and 1,4-dimethylcyclohexane.
[0040] The catalyst of the present invention is suitable for the following six-membered cycloalkane dehydrogenation reaction conditions: pressure 0.1-1.5 MPa, preferably 0.2-1.0 MPa, temperature 370-600°C, preferably 450-550°C, hydrogen / hydrocarbon volume ratio 300-2000, preferably 500-1500, raw material feed mass space velocity 0.1-20.0 h -1 , preferably 3 to 10 hours -1 .
[0041] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0042] In the examples and comparative examples, the specific surface area, pore volume and pore distribution of the carrier are determined by low-temperature N2 adsorption method, the specific surface area is calculated by BET method, the liquid nitrogen adsorption volume at a relative pressure (P / P0) of about 0.98 is taken as the total pore volume of the sample, and the pore size distribution is calculated according to SH / T0572-1993 method.
[0043] Example 1
[0044] The sulfate-containing γ-Al2O3 carrier of the present invention is prepared.
[0045] (1) Preparation of aluminum hydroxide powder containing sulfate
[0046] In a 3L stainless steel kettle, add 500mL of 200g / L sodium aluminate solution (with an alumina content of 62% by mass and a Na2O content of 37.5% by mass), add 10mL of 50g / L aluminum sulfate solution, adjust the pH of the slurry to 9.0, heat to 60°C, and carry out neutralization reaction for 30 minutes under sufficient stirring, then add 10mL of 20g / L sodium carbonate solution to adjust the pH value of the system to 9.6, continue stirring for 30 minutes to react, and then heat to 100°C for aging for 4 hours.
[0047] The aged slurry was filtered, and the obtained filter cake was washed with 30°C deionized water, with the amount of water used for each wash being 500 mL, for a total of 6 washes. The filter cake obtained from the last wash was dried at 120°C for 6 hours to obtain aluminum hydroxide powder containing sulfate, wherein the aluminum oxide content was 68% by mass.
[0048] (2) Preparation of Sulfate-Containing Alumina Support
[0049] 100 g of the aluminum hydroxide containing sulfate prepared in step (1) and 1.5 g of sesbania powder are mixed evenly to obtain a mixed powder, and a peptizing agent is prepared by using 68.0 ml of deionized water, 1 ml of nitric acid with a concentration of 68.0 mass%, 4 g of citric acid, and 4 ml of acetic acid with a concentration of 36 mass% and added to the mixed powder, wherein the mass ratio of the aluminum hydroxide containing sulfate: sesbania powder: nitric acid: acetic acid: citric acid: water is 100: 1.5: 0.95: 1.5: 4.0: 68. The mixed powder with the peptizing agent is kneaded evenly, extruded into strips through a perforated plate with a pore size of 2.0 mm, dried at 25° C. for 3 hours, dried at 120° C. for 12 hours, and calcined at 630° C. for 4 hours to obtain sulfate-containing γ-Al2O3.
[0050] The above-mentioned sulfate-containing γ-Al2O3 is placed in a reactor, the temperature is raised to 650°C, and 120°C water vapor (saturated steam pressure is 0.3MPa) is introduced for water vapor treatment at 650°C for 2 hours, the gas / solid volume ratio is 10:1, and the mass ratio of the water vapor to the sulfate-containing γ-Al2O3 is 1:200, to obtain the sulfate-containing γ-Al2O3 carrier Zt-1, in which the sulfate content is 0.6% by mass. The physical properties of the carrier are shown in Table 1.
[0051] Example 2
[0052] The sulfate-containing γ-Al2O3 carrier was prepared according to the method of Example 1, except that the concentration of the aluminum sulfate solution added to the aluminum hydroxide in step (1) was 60 g / L, the pH of the slurry was adjusted to 9.2, and after sufficient reaction at 60°C with stirring for 30 minutes, sodium carbonate solution was added to adjust the pH value of the system to 9.8. The aging temperature after the reaction was 120°C, and the aging time was 2 hours. (2) The sulfate-containing aluminum hydroxide prepared in step (1) was extruded, dried, and calcined to obtain sulfate-containing γ-Al2O3, which was heated to 660°C, and 120°C water vapor (saturated steam pressure 0.3 MPa) was introduced and steamed at 660°C for 2 hours, with a gas / solid volume ratio of 20:1, and the mass ratio of water vapor to sulfate-containing γ-Al2O3 was 1:100, to obtain sulfate-containing γ-Al2O3 carrier Zt-2, in which the sulfate content was 0.87% by mass. The physical properties of the carrier are shown in Table 1.
[0053] Example 3
[0054] Preparation of the catalyst of the present invention
[0055] Take 50 grams of the carrier Zt-1 prepared in Example 1, and prepare an impregnation solution with chloroplatinic acid, ammonium perrhenate, phosphoric acid, potassium chloride, citric acid and hydrochloric acid so that the impregnation solution contains 0.25% Pt, 0.25% Re, 0.30% P, 0.12% K, 1.8% Cl and 1.0% citric acid (all relative to the mass of alumina), and the liquid / solid volume ratio is 1.5. The carrier and the impregnation liquid were poured into a 500 ml flask, impregnated in a rotary vacuum evaporator (produced by Shanghai Yarong Biochemical Instrument Factory) at 25°C, 0.02 MPa, and a rotation speed of 0.03 m / s for 3 hours, the solid was dried under reduced pressure at 70°C, dried at 120°C for 12 hours, calcined in dry air at 500°C and a gas / agent volume ratio of 700 for 4 hours, and then reduced with H2 at 480°C and a gas / agent volume ratio of 500 for 4 hours to obtain catalyst Cat-1, whose composition is shown in Table 2.
[0056] Example 4
[0057] The catalyst of the present invention is prepared by a fractional impregnation method.
[0058] Take 50 grams of the carrier Zt-1 prepared in Example 1, prepare an impregnation solution with phosphoric acid and potassium chloride, so that the impregnation solution contains 0.30% P and 0.12% K (both relative to the mass of alumina), and the liquid / solid volume ratio is 1.5. Pour the carrier and the impregnation solution into a 500 ml flask, impregnate at 30°C for 3 hours, dry the impregnated solid at 120°C for 4 hours, and calcine in air at 500°C for 4 hours to obtain the Zt-1 carrier loaded with phosphorus and potassium.
[0059] Chloroplatinic acid, ammonium perrhenate, citric acid and hydrochloric acid were prepared into an impregnation solution, so that the impregnation solution contained 0.25% Pt, 0.25% Re, 1.8% Cl and 1.0% citric acid (all relative to the mass of alumina), and the liquid / solid volume ratio was 1.5. The Zt-1 carrier loaded with phosphorus and potassium and the impregnation solution were poured into a 500 ml flask, and impregnated for 3 hours in a rotary vacuum evaporator at 25°C, 0.02MPa, and a rotation speed of 0.03 m / s. The solid was dried under reduced pressure at 70°C and dried at 120°C for 12 hours. The catalyst was calcined in dry air at 500°C and a gas / agent volume ratio of 700 for 4 hours, and then reduced with H2 at 480°C and a gas / agent volume ratio of 500 for 4 hours to obtain the catalyst Cat-2, the composition of which is shown in Table 2.
[0060] Example 5
[0061] The catalyst was prepared according to the method of Example 3, except that the carrier used was the sulfate-containing γ-Al2O3 carrier ZT-2 prepared in Example 2, and chloroplatinic acid, ammonium perrhenate, phosphoric acid, potassium chloride, citric acid, and hydrochloric acid were prepared into an impregnation solution to make the impregnation solution contain 0.25% Pt, 0.25% Re, 0.40% P, 0.10% K, 1.8% Cl, and 1.0% citric acid (all relative to the mass of alumina). After the carrier was impregnated, dried, calcined, and reduced, a catalyst Cat-3 was obtained, the composition of which is shown in Table 2.
[0062] Example 6
[0063] The catalyst was prepared according to the method of Example 3, except that the carrier used was the sulfate-containing γ-Al2O3 carrier ZT-2 prepared in Example 2, and chloroplatinic acid, ammonium perrhenate, phosphorous acid, potassium chloride, citric acid and hydrochloric acid were prepared into an impregnation solution so that the impregnation solution contained 0.25% Pt, 0.42% Re, 0.30% P, 0.15% K, 1.8% Cl and 1.0% citric acid (all relative to the mass of alumina). After the carrier was impregnated, dried, calcined and reduced, a catalyst Cat-4 was obtained, the composition of which is shown in Table 2.
[0064] Comparative Example 1
[0065] The catalyst was prepared according to the method of Example 2 of CN1201715A.
[0066] (1) Preparation of carrier
[0067] Aluminum trichloride with a concentration of 4 g / 100 ml and ammonia water containing 6% (by weight) are added in calculated amounts, mixed evenly in a neutralization tank at a temperature of 60-80° C., and the pH is controlled to be 7.5-8.5; the generated aluminum hydroxide gel is filtered, washed with water, the filter cake is acidified with nitric acid, the acidified slurry is pelletized under pressure, the pellets aged in the pelletizing column are rinsed with water, and dried in an oven at 120-130° C. The obtained aluminum hydroxide pellets are calcined at 650-750° C. in an activation furnace for 4 hours, expanded with water vapor at a volume ratio of 0.2-1.0 at the same temperature for 12 hours, and sieved out after cooling. The carrier is obtained by mixing small γ-Al2O3 balls of mm in diameter.
[0068] (2) Preparation of Catalyst
[0069] Place 100 g of the carrier Al2O3 obtained in step (1) in an impregnator, and at the same time take 40 ml of chloroplatinic acid aqueous solution containing 0.01 g / ml of platinum; 11.4 ml of concentrated hydrochloric acid containing 37%; 29.3 ml of stannous chloride aqueous solution containing 0.025 g / ml of tin; 50.7 ml of potassium chloride aqueous solution containing 0.01 g / ml of potassium, add 50% ethanol aqueous solution so that the volume of the impregnation liquid is 0.8 times the volume of the carrier, and prepare an impregnation liquid. Add the above impregnation liquid to the impregnation device containing the Al2O3 carrier, impregnate evenly and then dry, then the small balls are calcined in a roasting furnace at an air flow rate of 1500 h. -1 , heated to 480-500℃, calcined at this temperature for 4 hours, then treated with air containing 30% water vapor at the same temperature for 4 hours, then stopped feeding water vapor and continued to dry and cool with air. Then reduced with hydrogen containing less than 20ppm of water at 480℃ for 2 hours to obtain a catalyst, denoted as DBCat-1, whose composition is shown in Table 2.
[0070] Comparative Example 2
[0071] The catalyst was prepared according to the method of Example 2 of CN110882703A.
[0072] (1) Preparation of carrier: Prepare 0.98M aluminum chloride solution, add magnesium sulfate calculated according to 110% of the theoretical sulfur requirement, and slowly add the aluminum chloride solution and ammonia solution into the gelling tank in parallel under stirring conditions, with the aluminum chloride flow rate of 2.0 ml / min. At the same time, add a solution containing a certain amount of titanium sulfate at a flow rate of 2.0 ml / min, and control the temperature in the gelling tank to 70°C and pH 8-10. After the gelling is completed, age for 0.5h, dry at 50°C under vacuum for 60h, and after forming, calcine at 700°C under nitrogen atmosphere for 6h to obtain the alumina carrier Mg-Ti-S / γ-Al2O3. The equivalent diameter of the obtained carrier is 0.5-2.0mm, and the specific surface area is 190-230m 2 / g, density is 0.55~0.70g / cm 3 .
[0073] (2) Impregnation aid component: According to the Sn content of the final catalyst of 1.0wt%, weigh an appropriate amount of tin tetrachloride to prepare an aqueous solution, and impregnate the Mg-Ti-S / γ-Al2O3 carrier therein. The solution is immersed at 70°C for 2h, then vacuum dried at 120°C for 2h, and calcined at 650°C for 4h to obtain the catalyst precursor Mg-Ti-S-Sn / γ-Al2O3.
[0074] (3) Impregnation of active metal components: Based on the Pt content of 0.6 wt% in the final catalyst, an appropriate amount of chloroplatinic acid was weighed to prepare an aqueous solution. The above-mentioned carrier was impregnated with the chloroplatinic acid solution by an equal volume impregnation method at 70°C for 6 h in vacuum, then vacuum dried at 120°C for 2 h, and calcined at 550°C for 4 h.
[0075] (4) Reduction: The product of step (3) is reduced with hydrogen as a reducing agent to obtain the catalyst, wherein the reduction temperature of the hydrogen is 530° C., the pressure is 0.1 MPa, and the volume flow rate of hydrogen per hour for reducing the catalyst is V H2 / V cat It is 1000:1.
[0076] The reduced catalyst is denoted as DBCat-2, which uses alumina containing Mg-Ti-S as a carrier, on which a Pt active metal component and an auxiliary component Sn are loaded. The composition of the catalyst is shown in Table 2.
[0077] Comparative Example 3
[0078] (1) Preparation of γ-Al2O3 carrier.
[0079] 100 g of pseudo-boehmite powder produced by alkoxyaluminum hydrolysis (produced by Sasol, Germany, brand SB, alumina content of 75% by mass) was mixed with 1.5 g of sesbania powder to obtain a mixed powder, and 68.0 ml of deionized water, 1 ml of nitric acid with a concentration of 68.0% by mass, 4 g of citric acid, and 4 ml of acetic acid with a concentration of 36% by mass were used to prepare a peptizing agent, which was added to the mixed powder. The mass ratio of the pseudo-boehmite: sesbania powder: nitric acid: acetic acid: citric acid: water was 100: 1.5: 0.95: 1.5: 4.0: 68. The mixed powder with the peptizing agent was kneaded evenly, extruded with a 2.0 mm orifice plate, dried at 25° C. for 3 hours, dried at 120° C. for 12 hours, and calcined in air at 630° C. for 4 hours to obtain the γ-Al2O3 carrier DBZt-1, whose physical properties are shown in Table 1.
[0080] (2) Preparation of Catalyst
[0081] Take 50 grams of carrier DBZt-1, prepare impregnation solution with chloroplatinic acid, ammonium perrhenate, phosphoric acid, potassium chloride, citric acid and hydrochloric acid, so that the impregnation solution contains 0.25% Pt, 0.25% Re, 0.40% P, 0.10% K, 1.8% Cl and 1.0% citric acid (all relative to the mass of alumina), and the liquid / solid volume ratio is 1.5. Pour the carrier and the impregnation solution into a 500 ml flask, impregnate for 3 hours in a rotary vacuum evaporator at 25°C, 0.02 MPa and a rotation speed of 0.03 m / s, dry the solid under reduced pressure at 70°C, and dry at 120°C for 12 hours. The catalyst was calcined in dry air at 500°C and a gas / agent volume ratio of 700 for 4 hours, and then reduced with H2 at 480°C and a gas / agent volume ratio of 500 for 4 hours. Thereafter, 0.16% (relative to the mass of the catalyst) of hydrogen sulfide was added to the hydrogen flow at 425°C to pre-sulfurize the catalyst to obtain catalyst DBCat-3, whose composition is shown in Table 2.
[0082] Example 7
[0083] 0.5 g of catalyst was loaded on the microreactor, and cyclohexane was used as the raw material to evaluate the dehydrogenation performance of the catalyst. The evaluation conditions were: 480°C, 0.85 MPa, and a feed mass space velocity of 4.0 h. -1 , hydrogen / hydrocarbon volume ratio 1000:1, reaction time 192 hours, dehydrogenation product is benzene, sampling and analysis are performed at regular intervals, and the evaluation results of each catalyst are shown in Table 3.
[0084] It can be seen from Table 3 that under the same reaction conditions, the catalyst of the present invention has a higher benzene yield than the catalyst prepared in the comparative example and remains stable for a long time, indicating that the catalyst has good selectivity and activity stability and a low carbon deposition rate.
[0085] Example 8
[0086] 35 g of catalyst was loaded on the medium-sized device, and the dehydrogenation performance of the catalyst was evaluated using methylcyclohexane as the raw material. The evaluation conditions were: 500°C, 0.35 MPa, and a feed mass space velocity of 8.0 h -1 , hydrogen / hydrocarbon volume ratio 1000:1, reaction time 192 hours, dehydrogenation product is toluene, sampling and analysis are performed at regular intervals, and the evaluation results of each catalyst are shown in Table 4, where the carbon deposit amount is the carbon deposit amount after 192 hours of reaction.
[0087] It can be seen from the data in Table 4 that under the reaction conditions of high space velocity and low pressure, the catalyst of the present invention has a higher toluene yield than the catalyst prepared in the comparative example and remains stable after a long reaction, indicating that the catalyst has good selectivity and activity stability and a low carbon deposition rate.
[0088] Example 9
[0089] Cat-1 and CatDB-3, which were deactivated by reacting for 192 hours under the conditions of Example 8, were charred at 400-450°C for 8 hours using air containing 0.5-1.0 volume % oxygen to obtain regenerated catalysts. The regenerated catalysts were evaluated according to the method of Example 8. The results are shown in Table 4.
[0090] From the data in Table 4, it can be seen that the catalyst Cat-1 of the present invention has better regeneration performance than the comparative catalyst CatDB-3.
[0091] Table 1
[0092]
[0093] Table 2
[0094]
[0095] Table 3
[0096]
[0097] Table 4
[0098]
Claims
1. A catalyst for dehydrogenating hexacyclic hydrocarbons to aromatic hydrocarbons, comprising an alumina carrier containing sulfate and components having the following contents calculated based on the alumina: The Group VIII metal is selected from platinum, the Group VIIB metal is selected from rhenium, the halogen is selected from chlorine, and the sulfate-containing aluminum oxide has the following pore radius distribution: pores with a pore radius of 3 to 5 nm account for 45 to 58% by volume of the total pore volume, pores with a pore radius of 5 to 10 nm account for 41 to 50% by volume of the total pore volume, and pores with a pore radius greater than 10 nm account for 1 to 8% by volume of the total pore volume; The preparation method of the sulfate-containing alumina carrier comprises the following steps: (1) Mixing a sodium aluminate solution and an aluminum sulfate solution, controlling the pH value thereof to 8.5 to 9.2, reacting at 50 to 80° C. for 0.3 to 1 hour, then adding a sodium carbonate solution to adjust the pH value of the system to 9.5 to 9.8, continuing the reaction for 0.3 to 1 hour, then heating to 98 to 150° C. for aging for 1.5 to 8 hours, washing the obtained solid with water, and drying to obtain aluminum hydroxide powder containing sulfate groups, (2) mixing aluminum hydroxide powder containing sulfate with a peptizing agent, extruding and forming strips, drying and calcining at 450-700° C. to obtain aluminum oxide containing sulfate, wherein the peptizing agent is an acid solution, wherein the acid is selected from one or more of hydrochloric acid, nitric acid, acetic acid and citric acid; (3) treating the sulfate-containing aluminum oxide with steam at 580-700° C. for 1-3 hours, wherein the gas / solid volume ratio is controlled to be 0.5-100:1 during the steam treatment, and the mass ratio of the steam to the sulfate-containing aluminum oxide is 1:80-300.
2. The catalyst according to claim 1, characterized in that The content of each component of the catalyst is:
3. The catalyst according to claim 1, characterized in that The aluminum oxide containing sulfate groups is γ-aluminum oxide containing sulfate groups.
4. The catalyst according to claim 1, characterized in that Sulfate-containing alumina has the following pore radius distribution: pores with a pore radius of 3 to 5 nm account for 45 to 55 volume % of the total pore volume, pores with a pore radius of 5 to 10 nm account for 41 to 48 volume % of the total pore volume, and pores with a pore radius greater than 10 nm account for 4 to 7 volume % of the total pore volume.
5. The catalyst according to claim 1, characterized in that The specific surface area of the sulfate-containing alumina carrier is 200 to 220 m 2 / g, pore volume is 0.6~0.9mL / g.
6. A method for preparing the catalyst according to claim 1, comprising impregnating an alumina carrier containing sulfate with a solution containing a Group VIII metal compound, a Group VIIB metal compound, a phosphorus-containing compound, a potassium-containing compound and a halogen as an impregnation liquid, and drying and calcining the impregnated solid.
7. A method for preparing the catalyst according to claim 1, comprising: (1) impregnating a sulfate-containing alumina carrier with a solution of a phosphorus-containing compound and a potassium-containing compound as an impregnation liquid, drying, and calcining; (2) The carrier calcined in step (1) is impregnated with a solution containing a Group VIII metal compound, a Group VIIB metal compound and a halogen as an impregnation solution, and the impregnated solid is dried and calcined.
8. The method according to claim 6 or 7, characterized in that The Group VIII metal compound is selected from chloroplatinic acid, tetraammonium dichloroplatinum, ammonium chloroplatinate, platinum trichloride, platinum tetrachloride hydrate, dicarbonyl platinum dichloride, dinitrodiaminoplatinum or sodium tetranitroplatinate.
9. The method according to claim 6 or 7, characterized in that The Group VIIB metal compound is selected from perrhenic acid or ammonium perrhenate.
10. The method according to claim 6 or 7, characterized in that The phosphorus-containing compound is selected from phosphoric acid, phosphorous acid or pyrophosphoric acid, the potassium-containing compound is selected from potassium chloride or potassium hydroxide, and the halogen is chlorine.
11. The method according to claim 6, characterized in that The impregnation solution contains a competitive adsorbent, and the competitive adsorbent is selected from one or more of hydrochloric acid, trichloroacetic acid, citric acid, acrylic acid and methanol.