A Pt-based catalyst and its application in catalytic reduction of hexavalent uranium to tetravalent uranium
The Pt/Al2O3-SiC catalyst prepared by using atomic layer deposition technology in acidic systems has solved the problem of low conversion rate of hexavalent uranium in the prior art, achieved efficient preparation of tetravalent uranium, and improved the reactivity of the catalyst and stability.
Patent Information
- Application Number
- CN202111234381.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-10-22
AI Technical Summary
The prior art has low efficiency in catalytic reduction of hexavalent uranium in acidic systems, and traditional catalyst preparation methods have problems such as uneven metal loading and easy loss of active components, resulting in a degradation of reaction performance.
The supported Pt/Al2O3-SiC catalyst is prepared on the Al2O3-SiC composite support by atomic layer deposition technology. The dispersion and reaction performance of the active metal are improved by atomic layer deposition. The specific steps include dispersing the Al2O3-SiC composite support in water-free In ethanol, atomic layer deposition treatment was performed, and a reduction reaction was performed in a kettle reactor.
Under acidic conditions, the conversion rate and reaction rate of hexavalent uranium are significantly improved, the conversion rate of U(VI) can reach 99%, and the reaction activity and stability of the catalyst are improved.
Smart Images

Figure BDA0003317217250000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nuclear fuel post-processing, and in particular to a catalyst for catalytic reduction of hexavalent uranium to prepare a tetravalent uranium solution, and a preparation method and application thereof. Background Art
[0002] Nuclear fuel reprocessing is an important part of the nuclear fuel cycle, and its purpose is to recover U, Pu and other valuable fission elements from spent fuel. At present, the Purex process is mainly used, in which the uranium-plutonium separation stage mainly uses the very small extraction capacity of tributyl phosphate for trivalent plutonium to achieve uranium-plutonium separation. At present, tetravalent uranium is mainly used as a reduction stripping agent, which has the advantages of complete plutonium reduction stripping, no introduction of impurities into the system, and fast reaction rate, and is widely used. Therefore, the preparation of tetravalent uranium is of great significance in the purex process.
[0003] At present, the main methods for preparing tetravalent uranium include electroreduction, photochemical method, high-pressure hydrogenation method, and organic reducing agent reduction method. The electrochemical method is to electrolyze UO2(NO3)2 to reduce it to U(NO3)4, but in the actual application process in the reprocessing plant, the conversion rate of hexavalent uranium (U(VI)) is low, generally only 50%-60%, which makes the concentration of tetravalent uranium (U(IV)) low. When it is used as a reducing agent, it will not only lead to the dilution of plutonium products, but also increase the recovery burden of uranium products. The photochemical method has the unique advantages of simple reaction system, easy control, easy maintenance and no residue of the reducing agent used. It is currently mostly used for the treatment of uranium-containing wastewater, and it is difficult to produce high-concentration tetravalent uranium. The high-pressure hydrogenation method has the characteristics of large production capacity and high U(IV) yield, but its equipment is complex, and the high-pressure hydrogen pressure used reaches 10MPa, which is a huge safety hazard for the highly radioactive nuclear fuel reprocessing workshop. The organic reducing agent reduction method refers to the use of organic reducing agents such as hydrazine, formic acid, and formaldehyde to reduce hexavalent uranium to tetravalent uranium under acidic conditions. It has the advantages of mild reaction conditions and simple preparation process. It is a very promising method for preparing U(VI).
[0004] Li Bin et al. used platinum black as a catalyst to study the process conditions of hydrazine reduction of U(VI) to U(IV) in a nitric acid system. When the uranium concentration was 0.9 mol / L, the HNO3 concentration was 0.8 mol / L, and the hydrazine concentration was 1 mol / L, the conversion rate of U(VI) could reach more than 90% at 60°C. Ananiev et al. summarized the application of organic reducing agent reduction in the preparation of tetravalent uranium (Heterogeneous catalytic redox reactions in the chemistry and technology of the nuclear fuel cycle). When hydrazine nitrate was used as a reducing agent, hexavalent uranium could be converted into tetravalent uranium using Pt / SiO2. However, the preparation methods such as impregnation method have the disadvantages of uneven metal loading, difficulty in accurately controlling the loading amount, easy secondary agglomeration of active metals, and easy loss of active components, resulting in decreased reaction performance. Compared with the traditional preparation methods of heterogeneous catalysts, atomic layer deposition technology has the advantages of controllable metal particle size at the atomic level, high dispersion, good reproducibility, and stronger interaction between metal and carrier, thereby improving the reaction performance of the catalyst. Summary of the invention
[0005] One of the technical problems to be solved by the present invention is to solve the problem of preparing U(IV) catalyst by catalytic reduction of U(VI) in an acidic system, and to provide a new catalyst which can obtain high reaction activity under mild conditions.
[0006] The second technical problem to be solved by the present invention is to adopt the method for preparing the catalyst described in the first technical problem above. The method utilizes the atomic layer deposition technology and can effectively improve the dispersion of the active metal.
[0007] The third technical problem to be solved by the present invention is to use the catalyst described in one of the above technical problems to realize the catalytic reaction process of catalytic reduction of U(VI) to prepare U(IV) under acidic conditions.
[0008] In order to solve one of the above technical problems, the present invention adopts the following technical solution:
[0009] With Pt as the active ingredient, an atomic layer deposition method is used to prepare a supported Pt / Al2O3-SiC catalyst on an Al2O3-SiC composite carrier; the mass percentage of Pt in the catalyst is 0.1%-5%; the mass percentage of Al2O3 in the Al2O3-SiC composite carrier is 5%-30%.
[0010] In order to solve the second of the above technical problems, the present invention adopts the following technical solution:
[0011] The preparation process of the Pt / Al2O3-SiC catalyst is to use an Al2O3-SiC composite carrier and an atomic layer deposition method to prepare the Pt / Al2O3-SiC catalyst; the specific steps are:
[0012] a) dispersing the Al2O3-SiC composite carrier in anhydrous ethanol, dispersing the carrier particles into a suspension by stirring or ultrasonic treatment, and then gradually evaporating the ethanol in the suspension to obtain a dried Al2O3-SiC sample; transferring the sample to an atomic layer deposition sample chamber, and purging the sample chamber and pipeline of the atomic layer deposition equipment with nitrogen;
[0013] b) Setting the parameters of atomic deposition as follows: using a room temperature liquid source metal Pt precursor MeCpPtMe3, the pulse, gas holding and gas extraction times of the precursor are 0.2-2s, 5-15s and 20-60s respectively; the pulse, gas holding and gas extraction times of O3 are 0.2-2s, 2-20s and 10-50s respectively; the Pt precursor and O3 are alternately introduced into the sample chamber, and the deposition cycle is 150-1500 times;
[0014] c) The obtained sample is taken out and subjected to reduction treatment to obtain the preparation of Pt / Al2O3-SiC catalyst.
[0015] The preparation process of Al2O3-SiC composite carrier is as follows:
[0016] The Al2O3-SiC composite carrier is prepared by an impregnation method. A soluble Al source is dissolved in deionized water to a concentration of 0.01 to 10 mol / L. A required amount of SiC carrier is taken, and the prepared Al source solution is added dropwise to the SiC carrier and mixed evenly. The mixture is then impregnated at room temperature for 8 to 16 hours and dried at 80 to 120°C for 4 to 24 hours. The mixture is then transferred to a muffle furnace and calcined at 300 to 500°C for 2 to 8 hours to obtain the Al2O3-SiC composite carrier.
[0017] The Al source is any one or two of Al(NO3)3 and AlCl3.
[0018] The reduction treatment process described in step (c) is that the reducing gas is H2, the molar purity is> 99.9%, and the volume space velocity of the reducing gas is 100-3600h -1 The heating rate from room temperature to the reduction temperature is 1-10°C / min, the reduction temperature is 200-600°C, the pressure is normal pressure, and the reduction time is 1-48h.
[0019] In order to solve the third of the above technical problems, the present invention adopts the following technical solution:
[0020] 1) The catalytic process is carried out in a tank reactor or a fixed bed reactor. The conditions for reducing hexavalent uranium to prepare a tetravalent uranium solution are: an acid concentration (in terms of hydrogen ion concentration) of 0.5-1.0 mol / L, a uranyl ion concentration of 100-300 g / L (in terms of uranium), a reducing agent concentration of 0.5-2.0 mol / L, a reaction temperature of 15-60° C., and a reaction pressure of normal pressure.
[0021] 2) The catalyst is used for catalytic reduction of hexavalent uranium to prepare tetravalent uranium in an acidic system.
[0022] 3) The reducing agent is any one, two or three of hydrazine nitrate, formic acid or formaldehyde.
[0023] 4) The acidic system is an acidic system formed by one or more of nitric acid, sulfuric acid or perchloric acid; the hexavalent uranium is a uranyl ion of the acid type corresponding to the acidic system, which is one or more of uranyl nitrate, uranyl sulfate and uranyl perchlorate solution; and the tetravalent uranium is a reduction product of the corresponding hexavalent uranium.
[0024] The advantages of the present invention are:
[0025] (1) The catalyst provided by the present invention has high dispersibility and high reaction activity.
[0026] (2) The catalyst provided by the present invention can reduce U(VI) to U(IV) solution under acidic conditions. Highly dispersed Pt species improve the conversion rate and reaction rate of U(VI). In a stirred tank reactor, the conversion rate of U(VI) can reach 99% within 30 minutes. DETAILED DESCRIPTION
[0027] The technical details of the present invention are described in detail by the following examples. It should be noted that the examples are only used to further illustrate the technical features of the present invention, rather than to limit the present invention.
[0028] Catalyst preparation and performance evaluation
[0029] Example 1
[0030] Take 0.654g AlCl3 and dissolve it in 5ml deionized water to prepare a solution. Take 4.75g SiC carrier, add the prepared Al solution to the SiC carrier and mix them evenly. Soak the mixture at room temperature for 12h and dry it at 120℃ for 12h. Then transfer it to a muffle furnace and calcine it at 500℃ for 4h to obtain a 5Al2O3-SiC composite carrier, in which the mass percentage of Al2O3 is 5%.
[0031] The prepared 5Al2O3-SiC composite carrier was ground and sieved, and 0.5g of the 200-300 mesh carrier was taken to prepare a Pt-based catalyst by atomic layer deposition. The 5Al2O3-SiC composite carrier was dispersed in 20ml of anhydrous ethanol, and the obtained particles were dispersed into a suspension by stirring (or ultrasonic treatment), and then the ethanol in the suspension was gradually evaporated to obtain a dried 5Al2O3-SiC sample. The sample was transferred to the atomic layer deposition sample chamber, and the sample chamber and pipeline of the atomic layer deposition equipment were cleaned with nitrogen; the parameters of atomic deposition were set as follows: the room temperature liquid source metal Pt precursor MeCpPtMe3 was used, and the pulse, holding and exhaust times of the precursor were 0.7s, 15s and 50s respectively. The pulse, holding and exhaust times of O3 were 0.6s, 12s and 30s respectively, and the Pt precursor and O3 were alternately introduced into the sample chamber, and the deposition cycle was 150 times. Catalyst reduction activation conditions: reducing gas is pure H2, molar purity> 99.9%, space velocity is 2000h -1 The heating rate from room temperature to the reduction temperature is 5°C / min, the reduction temperature is 300°C, the pressure is normal pressure, the reduction time is 1h, and a 0.5Pt / 5Al2O3-SiC catalyst with a Pt mass content of 0.5% is obtained.
[0032] The reaction conditions in the stirred tank were as follows: nitric acid concentration (in terms of hydrogen ion concentration) was 0.8 mol / L, uranyl ion (uranyl nitrate) concentration was 210 g / L, hydrazine nitrate concentration was 1.0 mol / L, temperature was 60°C, stirring rate was 800 rpm, pressure was normal pressure, catalyst dosage was 1.0 g, and reaction liquid was 25 mL. The reaction results are shown in Table 1.
[0033] Example 2
[0034] Take 3.676g Al(NO3)3·9H2O and dissolve it in 5ml deionized water to prepare a solution. Take 4.5g SiC carrier, add the prepared Al solution to the SiC carrier and mix them evenly. Soak the mixture at room temperature for 12h and dry it at 120℃ for 12h. Then transfer it to a muffle furnace and calcine it at 500℃ for 4h to obtain a 10Al2O3-SiC composite carrier, in which the mass percentage of Al2O3 is 10%.
[0035] The 10Al2O3-SiC composite carrier prepared above was ground and sieved, and 0.5g of the 200-300 mesh carrier was taken to prepare a Pt-based catalyst by atomic layer deposition. The 10Al2O3-SiC composite carrier was dispersed in 20ml of anhydrous ethanol, and the obtained particles were dispersed into a suspension by stirring or ultrasonic treatment, and then the ethanol in the suspension was gradually evaporated to obtain a dried 10Al2O3-SiC sample. The sample was transferred to the atomic layer deposition sample chamber, and the sample chamber and pipeline of the atomic layer deposition equipment were cleaned with nitrogen; the parameters of atomic deposition were set as follows: a room temperature liquid source metal Pt precursor MeCpPtMe3 was used, and the pulse, holding and exhaust times of the precursor were 0.7s, 15s and 50s respectively. The pulse, holding and exhaust times of O3 were 0.6s, 12s and 30s respectively, and the Pt precursor and O3 were alternately introduced into the sample chamber, and the deposition cycle was 900 times. Catalyst reduction activation conditions: reducing gas is pure H2, molar purity> 99.9%, space velocity is 2000h -1 The heating rate from room temperature to the reduction temperature is 5°C / min, the reduction temperature is 300°C, the pressure is normal pressure, the reduction time is 2h, and a 3Pt / 10Al2O3-SiC catalyst with a Pt mass content of 3% is obtained.
[0036] The reaction conditions in the stirred tank were as follows: nitric acid concentration (in terms of hydrogen ion concentration) was 0.8 mol / L, uranyl (uranyl nitrate) ion concentration was 210 g / L, hydrazine nitrate concentration was 1.0 mol / L, temperature was 60°C, stirring rate was 800 rpm, pressure was normal pressure, catalyst dosage was 1.0 g, and reaction liquid was 25 mL. The reaction results are shown in Table 1.
[0037] Example 3
[0038] Take 11.029g Al(NO3)3·9H2O and dissolve it in 20ml deionized water to prepare a solution. Take 3.5g SiC carrier, add the prepared Al solution to the SiC carrier and mix them evenly. Soak the mixture at room temperature for 12h and dry it at 120℃ for 12h. Then transfer it to a muffle furnace and calcine it at 500℃ for 4h to obtain a 30Al2O3-SiC composite carrier, in which the mass percentage of Al2O3 is 30%.
[0039] The prepared 30Al2O3-SiC composite carrier is ground and sieved, and 0.5g of the 200-300 mesh carrier is taken to prepare a Pt-based catalyst by atomic layer deposition. The 30Al2O3-SiC composite carrier is dispersed in 20ml of anhydrous ethanol, and the obtained particles are dispersed into a suspension by stirring or ultrasonic treatment, and then the ethanol in the suspension is gradually evaporated to obtain a dried 30Al2O3-SiC sample. The sample is transferred to the atomic layer deposition sample chamber, and the sample chamber and pipeline of the atomic layer deposition equipment are cleaned with nitrogen; the parameters of atomic deposition are set as follows: the room temperature liquid source metal Pt precursor MeCpPtMe3 is used, and the pulse, holding and exhaust times of the precursor are 0.7s, 15s and 50s respectively. The pulse, holding and exhaust times of O3 are 0.6s, 12s and 30s respectively, and the Pt precursor and O3 are alternately introduced into the sample chamber, and the deposition cycle is 1500 times. Catalyst reduction activation conditions: reducing gas is pure H2, molar purity> 99.9%, space velocity is 2000h -1 The heating rate from room temperature to the reduction temperature is 5°C / min, the reduction temperature is 400°C, the pressure is normal pressure, the reduction time is 3h, and a 5Pt / 30Al2O3-SiC catalyst with a Pt mass content of 5% is obtained.
[0040] The reaction conditions in the stirred tank were as follows: nitric acid concentration (in terms of hydrogen ion concentration) was 0.8 mol / L, uranyl (uranyl nitrate) ion concentration was 210 g / L, hydrazine nitrate concentration was 1.0 mol / L, temperature was 60°C, stirring rate was 800 rpm, pressure was normal pressure, catalyst dosage was 1.0 g, and reaction liquid was 25 mL. The reaction results are shown in Table 1.
[0041] Example 4
[0042] Take the 3Pt / 10Al2O3-SiC catalyst activated by reduction in Example 2. The reaction conditions in the stirred tank are as follows: sulfuric acid concentration (in terms of hydrogen ion concentration) is 1.0 mol / L, uranyl (uranyl sulfate) ion concentration is 210 g / L, hydrazine nitrate concentration is 1.0 mol / L, temperature is 60°C, stirring rate is 800 rpm, pressure is normal pressure, catalyst dosage is 1.0 g, and reaction liquid is 25 mL. The reaction results are shown in Table 1.
[0043] Example 5
[0044] Take the 3Pt / 10Al2O3-SiC catalyst activated by reduction in Example 2. The reaction conditions in the stirred tank are: perchloric acid concentration (in terms of hydrogen ion concentration) is 1.0 mol / L, uranyl (uranyl perchlorate) ion concentration is 210 g / L, hydrazine nitrate concentration is 1.0 mol / L, temperature is 60°C, stirring speed is 800 rpm, pressure is normal pressure, catalyst dosage is 1.0 g, and reaction liquid is 25 mL. The reaction results are shown in Table 1.
[0045] Example 6
[0046] Take the 3Pt / 10Al2O3-SiC catalyst activated by reduction in Example 2. The reaction conditions in the stirred tank are: nitric acid concentration (in terms of hydrogen ion concentration) is 1.0 mol / L, uranyl (uranyl nitrate) ion concentration is 210 g / L, formic acid concentration is 1.0 mol / L, temperature is 60°C, stirring speed is 800 rpm, pressure is normal pressure, catalyst dosage is 1.0 g, and reaction liquid is 25 mL. The reaction results are shown in Table 1.
[0047] Example 7
[0048] Take the 3Pt / 10Al2O3-SiC catalyst activated by reduction in Example 2. The reaction conditions in the stirred tank are: nitric acid concentration (in terms of hydrogen ion concentration) is 1.0 mol / L, uranyl (uranyl nitrate) ion concentration is 210 g / L, formaldehyde concentration is 1.0 mol / L, temperature is 60°C, stirring rate is 800 rpm, pressure is normal pressure, catalyst dosage is 1.0 g, and reaction liquid is 25 mL. The reaction results are shown in Table 1.
[0049] Example 8
[0050] Take the 3Pt / 10Al2O3-SiC catalyst activated by reduction in Example 2. Reaction conditions in the fixed bed: nitric acid concentration (in terms of hydrogen ion concentration) is 0.8 mol / L, uranyl (uranyl nitrate) ion concentration is 210 g / L, hydrazine nitrate concentration is 1.0 mol / L, temperature is 15°C, liquid space velocity is 0.3 h -1 , the pressure was normal pressure, the amount of catalyst was 20 g, and the flow rate of the reaction liquid was 0.1 ml / min. The reaction results are shown in Table 1.
[0051] Comparative Example 9
[0052] The Pt catalyst was prepared by impregnation method. Take 5.0g of the 10Al2O3-SiC carrier prepared in Example 2, weigh 0.399g H2PtCl6·6H2O and dissolve it in 5ml deionized water to prepare a mixed solution, the molar concentration of Pt is 0.154mol / L, add it dropwise to the 10Al2O3-SiC carrier and mix it evenly. Impregnate at room temperature for 12h, dry at 80℃ for 12h, and calcine at 300℃ in air atmosphere for 4h, wherein the mass content of Pt is 3%, recorded as 3Pt / 10Al2O3-SiC-IWI catalyst.
[0053] Catalyst reduction activation conditions: reducing gas is pure H2 (molar purity> 99.9%), space velocity is 2000h -1, heating rate is 5℃ / min, reduction temperature is 300℃, pressure is normal pressure, and reduction time is 2h. The reaction conditions for the catalyst in the stirred tank are: nitric acid concentration (in terms of hydrogen ion concentration) is 0.8mol / L, uranyl (uranyl nitrate) ion concentration is 210g / L, hydrazine nitrate concentration is 1.0mol / L, temperature is 60℃, stirring rate is 800rpm, pressure is normal pressure, catalyst dosage is 1.0g, and reaction liquid is 25mL. The reaction results are shown in Table 1.
[0054] Comparative Example 10
[0055] Take the Al2O3 carrier for grinding and sieving, take 0.5g of 200-300 mesh carrier, and prepare Pt-based catalyst by atomic layer deposition. Disperse the Al2O3 carrier in 20ml of anhydrous ethanol, disperse the obtained particles into a suspension by stirring or ultrasonic treatment, and then gradually evaporate the ethanol in the suspension to obtain a dried Al2O3 sample. Transfer this sample to the atomic layer deposition sample chamber, purge the sample chamber and pipeline of the atomic layer deposition equipment with nitrogen; set the parameters of atomic deposition as follows: use the room temperature liquid source metal Pt precursor MeCpPtMe3, and the pulse, hold and exhaust time of the precursor are 0.7s, 15s and 50s respectively. The pulse, hold and exhaust time of O3 are 0.6s, 12s and 30s respectively, and the Pt precursor and O3 are alternately introduced into the sample chamber, and the deposition cycle is 900 times. Catalyst reduction activation conditions: the reducing gas is pure H2, the molar purity is> 99.9%, and the air velocity is 2000h -1 The heating rate from room temperature to the reduction temperature is 5°C / min, the reduction temperature is 300°C, the pressure is normal pressure, the reduction time is 2h, and a 3Pt / Al2O3 catalyst with a Pt mass content of 3% is obtained.
[0056] The reaction conditions in the stirred tank were as follows: nitric acid concentration (in terms of hydrogen ion concentration) was 0.8 mol / L, uranyl (uranyl nitrate) ion concentration was 210 g / L, hydrazine nitrate concentration was 1.0 mol / L, temperature was 60°C, stirring rate was 800 rpm, pressure was normal pressure, catalyst dosage was 1.0 g, and reaction liquid was 25 mL. The reaction results are shown in Table 1.
[0057] Comparative Example 11
[0058] Take the SiC carrier for grinding and sieving, take 0.5g of 200-300 mesh carrier, and prepare Pt-based catalyst by atomic layer deposition. Disperse the SiC carrier in 20ml of anhydrous ethanol, disperse the obtained particles into a suspension by stirring or ultrasonic treatment, and then gradually evaporate the ethanol in the suspension to obtain a dried SiC sample. Transfer this sample to the atomic layer deposition sample chamber, clean the sample chamber and pipeline of the atomic layer deposition equipment with nitrogen; set the parameters of atomic deposition as follows: use room temperature liquid source metal Pt precursor MeCpPtMe3, the pulse, hold and exhaust time of the precursor are 0.7s, 15s and 50s respectively. The pulse, hold and exhaust time of O3 are 0.6s, 12s and 30s respectively, and the Pt precursor and O3 are alternately introduced into the sample chamber, and the deposition cycle is 900 times. Catalyst reduction activation conditions: the reducing gas is pure H2, the molar purity is> 99.9%, and the air velocity is 2000h -1 The heating rate from room temperature to the reduction temperature is 5°C / min, the reduction temperature is 300°C, the pressure is normal pressure, the reduction time is 2h, and a 3Pt / SiC catalyst with a Pt mass content of 3% is obtained.
[0059] The reaction conditions in the stirred tank were as follows: nitric acid concentration (in terms of hydrogen ion concentration) was 0.8 mol / L, uranyl (uranyl nitrate) ion concentration was 210 g / L, hydrazine nitrate concentration was 1.0 mol / L, temperature was 60°C, stirring rate was 800 rpm, pressure was normal pressure, catalyst dosage was 1.0 g, and reaction liquid was 25 mL. The reaction results are shown in Table 1.
[0060] Table 1 Reaction performance of hydrazine reduction of hexavalent uranium to tetravalent uranium under acidic conditions on different catalysts
[0061]
[0062] As shown in Table 1, the activity of 3Pt / 10Al2O3-SiC catalyst prepared by atomic layer deposition in the catalytic reduction of hexavalent uranium to tetravalent uranium is significantly higher than that of 3Pt / 10Al2O3-SiC-IWI catalyst prepared by impregnation method. The above experimental results show that atomic layer deposition method has advantages and improves the reaction performance of the catalyst. However, when a single carrier such as Al2O3 or SiC carrier is used to prepare the catalyst, the U(VI) conversion rate is only about 60%, which is significantly lower than that of the composite carrier catalyst. This shows that composite carriers are crucial for the preparation of highly active Pt-based catalysts.
Claims
1. A Pt-based catalyst, Features: With Pt as the active ingredient, 2 O 3 Supported Pt / Al was prepared by atomic layer deposition on SiC composite support 2 O 3 -SiC catalyst; the mass percentage of Pt in the catalyst is 0.1%-5%; the Al 2 O 3 Al-SiC composite support 2 O 3 The mass percentage is 5%-30%; Pt / Al 2 O 3 -SiC catalyst preparation process is to use Al 2 O 3 -SiC composite support, prepared by atomic layer deposition of Pt / Al 2 O 3 -SiC catalyst; the specific steps are: a) Al 2 O 3 -SiC composite carrier is dispersed in anhydrous ethanol, and the carrier particles are dispersed into a suspension by stirring or ultrasonic treatment, and then the ethanol in the suspension is gradually evaporated to obtain the dried Al 2 O 3 -SiC samples; The sample is transferred to an atomic layer deposition sample chamber, and the sample chamber and pipelines of the atomic layer deposition equipment are purged with nitrogen; b) Setting the atomic deposition parameters: using room temperature liquid source metal Pt precursor MeCpPtMe 3 The pulse, breath holding and breath extraction times of the precursor are 0.2-2 s, 5-15 s and 20-60 s respectively; 3 The pulse, breath holding and air extraction times were 0.2-2 s, 2-20 s and 10-50 s, respectively. Pt precursor and O were introduced into the sample chamber alternately. 3 , cycle deposition 150-1500 times; c) After the obtained sample is taken out and reduced, Pt / Al 2 O 3 -SiC catalyst; Al 2 O 3 -The preparation process of SiC composite carrier is as follows: Al was prepared by impregnation method 2 O 3 -SiC composite carrier, dissolve a soluble Al source in deionized water to a concentration of 0.01-10 mol / L; take a required amount of SiC carrier, drop the prepared Al source solution into the SiC carrier, and mix them evenly; then soak the mixture at room temperature for 8-16 h, dry it at 80-120 °C for 4-24 h; then transfer it to a muffle furnace and calcine it at 300-500 °C for 2-8 h to obtain Al 2 O 3 -SiC composite carrier.
2. The Pt-based catalyst according to claim 1, Features: The Al source is Al(NO 3 ) 3 、AlCl 3 Any one or two of the following.
3. The Pt-based catalyst according to claim 1, Features: The reduction process described in step (c) is that the reducing gas is H 2 , molar purity>99.9%, volume space velocity of reducing gas is 100-3600 h -1 The heating rate from room temperature to the reduction temperature is 1-10 ℃ / min, the reduction temperature is 200-600 ℃, the pressure is normal pressure, and the reduction time is 1-48 h.
4. Use of a Pt-based catalyst according to any one of claims 1 to 3, Features: The catalyst is used for catalytic reduction of hexavalent uranium to prepare tetravalent uranium in an acidic system.
5. The use according to claim 4, Features: The reducing agent is any one, two or three of hydrazine nitrate, formic acid or formaldehyde.
6. The use according to claim 4, Features: The acidic system is an acidic system formed by one or more of nitric acid, sulfuric acid or perchloric acid; the hexavalent uranium is a uranyl ion of the acid type corresponding to the acidic system, which is one or more of uranyl nitrate, uranyl sulfate and uranyl perchlorate solution; and the tetravalent uranium is a reduction product of the corresponding hexavalent uranium.
7. The use according to any one of claims 4 to 6, Features: The catalytic process is carried out in a kettle reactor or a fixed bed reactor. The conditions for reducing hexavalent uranium to prepare tetravalent uranium solution are: acid concentration is 0.5-1.0 mol / L, the acid concentration is measured in terms of hydrogen ion concentration; uranyl ion concentration is 100-300 g / L, the uranyl ion concentration is measured in terms of uranium; the concentration of the reducing agent is 0.5-2.0 mol / L, the reaction temperature is 15-60 °C, and the reaction pressure is normal pressure.