A kind of hemming adhesive for automobile, preparation method and application

By combining polyethersulfone modified bisphenol A epoxy resin with other modified epoxy resins in automotive edging glue, a crosslinked structure is formed, which solves the dissolution and impact peeling properties of edging glue in phosphating liquid. The problem of insufficient results has achieved higher dissolution resistance and impact peeling strength, and improved the overall mechanical properties.

CN116004160BActive Publication Date: 2024-11-26TIANJIN JINGDABAOGUANG AUTOMOBILE SPARE PART CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211708076.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-11-26
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing automotive edge glue dissolves slag in the phosphating liquid, affecting subsequent processes, and insufficient impact peeling performance, affecting bonding reliability.

Method used

Bisphenol A epoxy resin modified with polyether sulfone and polyurethane modified epoxy resin, polyether modified epoxy resin, curing agent, curing accelerator, carbon black, thixotropic agent, moisture absorbent, wollastonite powder and Combination of flame retardants and other combinations form a dual crosslinking structure and crosslinking network, improve toughness and impact resistance, and use wollastonite powder to replace heavy calcium carbonate to prevent dissolution.

Benefits of technology

The dissolution resistance and impact peeling properties of the folded edge glue are significantly improved, and its mechanical properties and polar solvent resistance are enhanced, which avoids dissolution and slag dropping phenomena, while improving the shear strength and T peeling strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004024659310000121
    Figure BDA0004024659310000121
  • Figure BDA0004024659310000131
    Figure BDA0004024659310000131
  • Figure BDA0004024659310000141
    Figure BDA0004024659310000141
Patent Text Reader

Abstract

The present invention provides a kind of automotive hemming glue, preparation method and application, the automotive hemming glue comprises the following raw materials in parts by weight: 40-50 parts of epoxy resin, 2-5 parts of polyethersulfone, 2-5 parts of curing agent, 0.5-1.5 parts of curing accelerator, 1.5-5 parts of epoxy toughener, 3-5 parts of carbon black, 3-5 parts of thixotropic agent, 3-5 parts of moisture absorbent, 20-30 parts of wollastonite powder, 3-5 parts of glass microbeads, and 5-10 parts of optional flame retardant; the epoxy resin comprises 20-30 parts of bisphenol A epoxy resin, 15-20 parts of polyurethane modified epoxy resin, and 3-5 parts of polyether modified epoxy resin. The automotive hemming glue has good corrosion resistance and impact peeling performance, and is particularly suitable for the hemming parts of car doors, engine hoods or trunk lids.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile sealants, in particular to the technical field of epoxy resin adhesives. Background Art

[0002] After the inner and outer panels of the car door, engine hood, trunk lid (back door) are hemmed, they need to be folded and glued, which can not only strengthen the structure, seal the car body, improve the safety performance of the car body collision and extend the life of the car body. At the same time, using glue instead of welding can also reduce the problem of car body pits caused by welding and ensure the smoothness and beauty of the car body. If the product uses galvanized steel plates, the welding connection method will also damage the zinc layer around the welding part, resulting in reduced anti-corrosion performance of the product. Therefore, using glue instead of welding can also effectively solve the rust caused by the destruction of the zinc layer. At the same time, it can also prevent the premature rust of the bonding part due to the inability to paint.

[0003] Hemming adhesives can be divided into epoxy resin, polyvinyl chloride and polyacrylate according to different base materials. Epoxy resin hemming adhesives are widely used in automobile manufacturing companies because of their high strength, no corrosive gas generated when decomposed by heat and good corrosion resistance.

[0004] As a structural adhesive on the automobile assembly line, hemming glue is specifically used in welding workshops for structural bonding before degreasing, and then enters the pre-treatment process, that is, the entire car body is immersed in the treatment liquid for surface treatment. The general process currently used for surface treatment is: degreasing → water washing → surface adjustment → phosphating → water washing. Phosphating refers to immersing the entire car body in the phosphating solution. The main component of the phosphating solution is dihydrogen phosphate, which is acidic. The existing hemming glue filler generally contains a large amount of heavy calcium carbonate, which is easy to dissolve and drop in the phosphating solution, affecting the rhythm of subsequent processes. In addition, although the current hemming glue has high shear and T-peel strength, its impact peeling performance is poor, which will seriously affect the reliability of the hemming glue bonding.

[0005] Therefore, it is necessary to develop a hemming adhesive that is both resistant to corrosion and has high impact strength. Summary of the invention

[0006] In view of the above-mentioned defects or deficiencies in the prior art, the present application aims to provide an automotive hem glue having good corrosion resistance and good impact peeling performance, a preparation method and application.

[0007] One of the purposes of the present invention is to provide an automotive hem glue, comprising the following raw materials in parts by weight: 40 to 50 parts of epoxy resin, 2 to 5 parts of polyether sulfone, 2 to 5 parts of curing agent, 0.5 to 1.5 parts of curing accelerator, 1.5 to 5 parts of epoxy toughening agent, 3 to 5 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 5 parts of hygroscopic agent, 20 to 30 parts of wollastonite powder, 3 to 5 parts of glass microspheres, and 5 to 10 parts of flame retardant.

[0008] The epoxy resin comprises 20-30 parts of bisphenol A epoxy resin, 15-20 parts of polyurethane modified epoxy resin, and 3-5 parts of polyether modified epoxy resin.

[0009] Furthermore, the automotive hemming adhesive comprises the following raw materials in parts by weight: 22 to 26 parts of bisphenol A epoxy resin, 15 to 18 parts of polyurethane modified epoxy resin, 3-4 parts of polyether modified epoxy resin, 2 to 4 parts of polyether sulfone, 3 to 4.5 parts of curing agent, 0.5 to 1 part of curing accelerator, 2 to 2.5 parts of epoxy toughening agent, 3 to 4 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 4 parts of hygroscopic agent, 23 to 27 parts of wollastonite powder, 3 to 3.5 parts of glass beads, and 6 to 8 parts of flame retardant.

[0010] Preferably, the bisphenol A epoxy resin is a liquid bisphenol A epoxy resin, preferably a liquid bisphenol A epoxy resin having a viscosity of 11000 to 40000 mPa·s and an epoxy equivalent of 180 to 250 g / eq, and more preferably one or more of E44, E51 or YD128.

[0011] Preferably, the viscosity of the polyurethane-modified epoxy resin is 13000 to 23000 mPa·s, and the epoxy equivalent is 230 to 260 g / eq.

[0012] Preferably, the polyurethane modified epoxy resin is complex high-tech EPU133L.

[0013] Preferably, the viscosity of the polyether-modified epoxy resin is 20,000 to 30,000 mPa·s, and the epoxy equivalent is 600 to 700 g / eq. The viscosity of the polyether-modified epoxy resin is preferably 25,000 mPa·s, and the epoxy equivalent is preferably 630 g / eq.

[0014] Preferably, the polyether-modified epoxy resin is complex high-tech EP-1307.

[0015] Preferably, the polyethersulfone is an ultrafine powder of 80 to 500 meshes.

[0016] Preferably, the polyethersulfone is Solvay 3000P from the United States.

[0017] Preferably, the curing agent comprises one or a combination of dicyandiamide, sebacic acid dihydrazide or adipic acid dihydrazide, preferably dicyandiamide.

[0018] Preferably, the curing accelerator is an organic urea accelerator, preferably HUA5050 and / or HUA5200.

[0019] Preferably, the particle size of the wollastonite powder is 10-20 μm, preferably 15 μm.

[0020] Preferably, the wollastonite powder is GY-800 produced by Guangyuan Chemical.

[0021] Preferably, the viscosity of the epoxy toughening agent is 2000-4500 mPa·s.

[0022] Preferably, the epoxy toughening agent is Dow FORTEGRA 100 and / or Yike FORTEGRA 100.

[0023] Preferably, the moisture absorbent is calcium oxide.

[0024] Preferably, the thixotropic agent includes one or more of nano calcium carbonate, organic bentonite or kaolin, preferably nano calcium carbonate, and more preferably nano calcium carbonate having a particle size of less than 100 nm.

[0025] Preferably, the carbon black is conductive carbon black.

[0026] Preferably, the particle size of the glass microbeads is 150-200 μm.

[0027] Preferably, the flame retardant includes one or a combination of aluminum hydroxide, ammonium polyphosphate or red phosphorus flame retardant, preferably aluminum hydroxide.

[0028] The second object of the present invention is to provide a method for preparing an automotive hemming adhesive, which comprises first modifying bisphenol A epoxy resin with polyethersulfone, and then uniformly mixing the polyethersulfone-modified bisphenol A epoxy resin with polyurethane-modified epoxy resin, polyether-modified epoxy resin, curing agent, curing accelerator, epoxy toughening agent, carbon black, thixotropic agent, hygroscopic agent, wollastonite powder, glass beads and flame retardant.

[0029] Preferably, the preparation method of polyethersulfone-modified bisphenol A epoxy resin comprises: heating bisphenol A epoxy resin to 70-90° C., adding polyethersulfone at least three times, stirring for 40-90 minutes after each addition of polyethersulfone, and cooling when the epoxy resin becomes a uniform and transparent state.

[0030] Preferably, the preparation method of the automotive hemming adhesive comprises: mixing wollastonite powder, flame retardant, carbon black and polyethersulfone-modified bisphenol A epoxy resin, and stirring for 20 to 60 minutes; adding thixotropic agent, hygroscopic agent, curing agent, curing accelerator, polyurethane-modified epoxy resin and polyether-modified epoxy resin, and stirring for 20 to 60 minutes; adding glass microbeads and epoxy toughening agent, scraping the wall several times and stirring until there are no powder particles; vacuuming, stirring and degassing for 40 to 90 minutes.

[0031] The third object of the present invention is to provide an application of automotive hemming glue as automotive sealant

[0032] Preferably, the automotive hemming adhesive is used for hemming areas of vehicle doors, engine hoods or trunk lids.

[0033] The beneficial effects of the present invention include:

[0034] 1. Use bisphenol A epoxy resin modified with polyethersulfone to form a double cross-linked structure during the curing process, which effectively improves the toughness of the epoxy resin.

[0035] 2. Control the reaction rate of epoxy resin chemical crosslinking by controlling the amount of curing agent and curing accelerator added to form a uniformly structured crosslinking network, so that the toughness and impact resistance of the cured epoxy resin system are stronger.

[0036] 3. The use of polyurethane modified epoxy resin is beneficial to form a structurally uniform cross-linked network between polyethersulfone and epoxy resin, further enhancing the toughness of epoxy resin.

[0037] 4. The use of polyether-modified epoxy resin can increase the flexibility of epoxy resin, enhance impact resistance and fracture toughness, play an anti-static role, and enhance the polar solvent resistance of epoxy resin.

[0038] 5. Epoxy toughening agent is used to increase the toughness of epoxy resin after curing. It can improve the toughness and impact resistance of epoxy resin system without affecting the curing rate, modulus and chemical resistance of epoxy system.

[0039] 6. The use of carbon black and thixotropic agent can adjust the thixotropy of the composition, which is beneficial to improve the fluidity of processing and operability during use.

[0040] 7. Use wollastonite powder to completely replace heavy calcium carbonate as filler. First, it can prevent the cured hemming glue from dissolving and falling off in the treatment liquid; second, the wollastonite forms a three-dimensional structure that intersects with each other, which can improve the toughness and impact resistance of the hemming glue; third, wollastonite can enhance the dimensional stability of the material, and improve the tensile strength, tensile modulus, heat deformation temperature and creep resistance.

[0041] 8. In order to make wollastonite powder more easily dispersed in epoxy resin, the present invention uses polyethersulfone-modified bisphenol A epoxy resin, polyurethane-modified epoxy resin and polyether-modified epoxy resin to increase the compatibility of wollastonite powder and epoxy resin. DETAILED DESCRIPTION

[0042] In the following description, certain specific details are included to provide a comprehensive understanding of each disclosed embodiment. However, one skilled in the relevant art will recognize that the embodiments can be implemented without one or more of these specific details, but with other methods, components, materials, etc.

[0043] Unless otherwise required in this application, throughout the specification and the claims that follow, the words "including" and "comprising" should be interpreted in an open, inclusive sense, ie, "including, but not limited to."

[0044] References to "one embodiment" or "an embodiment" or "a preferred embodiment" or "certain embodiments" throughout this specification mean that the specific referenced elements, structures or features described in connection with the embodiment are included in at least one embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" or "in a preferred embodiment" or "in certain embodiments" appearing in different places throughout the specification do not necessarily all refer to the same embodiment. In addition, the specific elements, structures or features may be combined in any appropriate manner in one or more embodiments.

[0045] According to a first aspect of the present invention, there is provided an automotive hem glue, comprising the following raw materials in parts by weight: 40 to 50 parts of epoxy resin, 2 to 5 parts of polyethersulfone, 2 to 5 parts of curing agent, 0.5 to 1.5 parts of curing accelerator, 1.5 to 5 parts of epoxy toughening agent, 3 to 5 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 5 parts of hygroscopic agent, 20 to 30 parts of wollastonite powder, 3 to 5 parts of glass microspheres, and 5 to 10 parts of flame retardant.

[0046] The epoxy resin comprises 20-30 parts of bisphenol A epoxy resin, 15-20 parts of polyurethane modified epoxy resin, and 3-5 parts of polyether modified epoxy resin.

[0047] In the present invention, the epoxy resin is, for example, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts or 50 parts.

[0048] After cross-linking and curing, epoxy resin has strong adhesion, strong chemical corrosion resistance, and high mechanical strength, and is particularly suitable for bonding metal materials, but the toughness of the material is not high and the impact resistance is not good. Therefore, in the present invention, the bisphenol A epoxy resin uses a bisphenol A epoxy resin modified with polyether sulfone, and the impact strength of the bisphenol A epoxy resin system can be improved by adding polyether sulfone. Polyether sulfone is a thermoplastic polymer material, and the ether bond in its structure can both improve the toughness of the epoxy resin and not reduce the heat resistance and rigidity of the epoxy resin.

[0049] Bisphenol A epoxy resin modified by polyethersulfone will form a double cross-linked structure during the curing process. The double cross-linked structure includes physical cross-links formed between polyethersulfone and epoxy resin due to molecular entanglement and chemical cross-links between epoxy resins. The two cross-links form a semi-interpenetrating cross-linked network, which restricts the movement of molecules, thereby effectively improving the toughness of the epoxy resin.

[0050] The chemical cross-linking process of the epoxy resin will restrict the movement of the polyethersulfone molecules, resulting in uneven cross-linking density. In order to maintain good fluidity of the polyethersulfone during the formation of the two cross-linking structures, the present invention also controls the reaction speed of the epoxy resin chemical cross-linking by controlling the addition amount of the curing agent and the curing accelerator to form a cross-linking network with a uniform structure, so that the toughness and impact resistance of the epoxy resin system after curing are stronger.

[0051] Wherein, the bisphenol A epoxy resin is, for example, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.

[0052] When the amount of polyethersulfone added is less than 2 parts or greater than 5 parts, the modification effect on the bisphenol A epoxy resin is not obvious. Therefore, in the present invention, the amount of polyethersulfone added is 2 to 5 parts, for example, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts.

[0053] When the curing agent is less than 2 parts or the curing accelerator is less than 0.5 parts, the required curing time is too long, affecting the production cycle. When the curing agent is greater than 5 parts or the curing accelerator is greater than 1.5 parts, the curing reaction is too fast, making the toughness and impact resistance of the epoxy resin relatively weak. Therefore, the addition amount of the curing agent is 2 to 5 parts, for example, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts; the addition amount of the curing accelerator is 0.5 to 1.5 parts, for example, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts or 1.5 parts.

[0054] Polyurethane modified epoxy resin refers to polyurethane grafted epoxy resin, which forms an epoxy resin-polyurethane interpenetrating polymer network structure or island structure after curing, thereby improving the toughness of epoxy resin materials, improving the shear strength, adhesion, tensile strength, bending strength, wear resistance, etc. of the epoxy resin adhesive layer after curing, and at the same time, having little effect on the heat resistance of the material. At the same time, the polyurethane modified epoxy resin can have good fluidity during the curing process, can delay the gel time, and is conducive to the formation of a cross-linked network with uniform structure between polyether sulfone and epoxy resin. In the present invention, the addition amount of polyurethane modified epoxy resin is 15 to 20 parts, for example, 15 parts, 15.5 parts, 16 parts, 16.5 parts, 17 parts, 17.5 parts, 18 parts, 18.5 parts, 19 parts, 19.5 parts or 20 parts.

[0055] Polyether-modified epoxy resin refers to embedding polyether in the epoxy resin molecular chain. The embedding of polyether groups can replace long-chain aliphatic compounds, increase the flexibility of epoxy resin, and enhance impact resistance and fracture toughness; secondly, it makes the ion mobility in the epoxy resin molecules stronger, which plays an antistatic role; thirdly, the embedding of polar polyether groups can increase the absorption of epoxy resin in polar solvents, and the resistance to polar solvents is enhanced. In the present invention, the addition amount of the polyether-modified epoxy resin is 3-5 parts, for example, 3 parts, 3.2 parts, 3.5 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0056] In the present invention, the epoxy toughening agent is used to increase the toughness of the epoxy resin after curing, and can improve the toughness and impact resistance of the epoxy resin system without affecting the curing rate, modulus and chemical resistance of the epoxy system. The epoxy toughening agent is added in an amount of 1.5 to 5 parts, for example, 1.5 parts, 1.8 parts, 2 parts, 2.3 parts, 2.5 parts, 2.8 parts, 3 parts, 3.2 parts, 3.5 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0057] In the present invention, carbon black is mainly used for color adjustment and adjusting the thixotropy of the composition, which is beneficial to improving the fluidity during processing and the operability during use. The added amount of the carbon black is 3 to 5 parts, for example, 3 parts, 3.2 parts, 3.5 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0058] In the present invention, the thixotropic agent is, for example, 3 parts, 3.2 parts, 3.5 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0059] In the present invention, the moisture absorbent is, for example, 3 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0060] Wollastonite is a chain-like metasilicate mineral belonging to the triclinic system. It can not only maintain its needle-like and fibrous structure in the state of small particles, but also has the characteristics of high aspect ratio and strong anisotropy. In the present invention, wollastonite powder is used to completely replace heavy calcium carbonate as filler. On the one hand, it can prevent the cured hemming glue from dissolving in the treatment liquid; on the other hand, the wollastonite with a needle-like structure forms a mutually intersecting three-dimensional structure during the stacking process of the filler, which cooperates with the three-dimensional network structure formed by the epoxy resin during the cross-linking and curing process, thereby improving the toughness and impact resistance of the hemming glue; on the third hand, wollastonite has a low thermal expansion coefficient, and filling it into epoxy resin can enhance the dimensional stability of the material, and improve the tensile strength, tensile modulus, heat deformation temperature and creep resistance; on the fourth hand, since the surface of wollastonite is polar, its dispersion performance is poor when compounded with organic polymer materials, which can easily affect the mechanical properties of the material. Therefore, the present invention uses polyethersulfone-modified bisphenol A epoxy resin, polyurethane-modified epoxy resin and polyether-modified epoxy resin to increase the compatibility of wollastonite powder with epoxy resin, so that wollastonite powder is easier to disperse in epoxy resin. When the amount of wollastonite powder added is greater than 30 parts or less than 20 parts, the bonding properties and mechanical properties of the cured epoxy resin are poor. Therefore, in the present invention, the amount of wollastonite powder added is 20 to 30 parts, for example, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.

[0061] In the present invention, the glass beads are used to control the gap size between the two steel plates that need to be bonded during construction, that is, the thickness of the hemming glue between the two steel plates after construction is approximately equal to the diameter of the glass beads. When the amount of glass beads added is greater than 3 parts or less than 5 parts, the thickness of the hemming glue is uneven. The amount of glass beads added is 3 to 5 parts, for example, 3 parts, 3.2 parts, 3.5 parts, 3.7 parts, 4 parts, 4.2 parts, 4.5 parts, 4.7 parts or 5 parts.

[0062] In the present invention, the flame retardant is, for example, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts.

[0063] In a preferred embodiment of the present invention, the automotive hemming adhesive comprises the following raw materials in parts by weight: 22 to 26 parts of bisphenol A epoxy resin, 15 to 18 parts of polyurethane modified epoxy resin, 3-4 parts of polyether modified epoxy resin, 2 to 4 parts of polyether sulfone, 3 to 4.5 parts of curing agent, 0.5 to 1 part of curing accelerator, 2 to 2.5 parts of epoxy toughening agent, 3 to 4 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 4 parts of hygroscopic agent, 23 to 27 parts of wollastonite powder, 3 to 3.5 parts of glass beads, and 6 to 8 parts of flame retardant.

[0064] In a preferred embodiment of the present invention, the bisphenol A epoxy resin is a liquid bisphenol A epoxy resin, preferably a liquid bisphenol A epoxy resin with a viscosity of 11000 to 40000 mPa·s and an epoxy equivalent of 180 to 250 g / eq, and more preferably one or more of E44, E51 or YD128.

[0065] In the present invention, the viscosity of the bisphenol A epoxy resin is, for example, 11000, 15000, 19000, 22000, 26000, 30000, 33000, 36000 or 40000 mPa·s.

[0066] The bisphenol A epoxy resin has an epoxy equivalent of, for example, 180, 190, 200, 210, 220, 230, 240 or 250 g / eq.

[0067] The bisphenol A epoxy resin is, for example, E44, E51, YD128, E44 and E51, E44 and YD128, E51 and YD128, or a combination of E44, E51 and YD128.

[0068] Preferably, the viscosity of the polyurethane-modified epoxy resin is 13000 to 23000 mPa·s, and the epoxy equivalent is 230 to 260 g / eq.

[0069] In the present invention, the viscosity of the polyurethane-modified epoxy resin is, for example, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000 or 23,000 mPa·s.

[0070] The epoxy equivalent of the polyurethane-modified epoxy resin is, for example, 230, 235, 240, 245, 250, 255 or 260 g / eq.

[0071] The polyurethane modified epoxy resin is preferably complex high-tech EPU133L.

[0072] Preferably, the viscosity of the polyether-modified epoxy resin is 20,000 to 30,000 mPa·s, and the epoxy equivalent is 600 to 700 g / eq.

[0073] In the present invention, the viscosity of the polyether-modified epoxy resin is, for example, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000 or 30,000 mPa·s.

[0074] The epoxy equivalent of the polyether-modified epoxy resin is, for example, 600, 610, 620, 630, 640, 650, 660, 670, 680, 690 or 700 g / eq.

[0075] The viscosity of the polyether-modified epoxy resin is preferably 25000 mPa·s, and the epoxy equivalent is preferably 630 g / eq.

[0076] Preferably, the polyether-modified epoxy resin is complex high-tech EP-1307.

[0077] In a preferred embodiment of the present invention, the polyethersulfone is an ultrafine powder of 80-500 mesh.

[0078] In the present invention, the polyethersulfone is, for example, 80 mesh, 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh, 350 mesh, 400 mesh, 450 mesh, or 500 mesh.

[0079] Preferably, the polyethersulfone is Solvay 3000P from the United States.

[0080] Preferably, the curing agent includes one or more of dicyandiamide, sebacic acid dihydrazide or adipic acid dihydrazide.

[0081] In the present invention, the curing agent is, for example, dicyandiamide, sebacic acid dihydrazide, adipic acid dihydrazide, dicyandiamide and sebacic acid dihydrazide, dicyandiamide and adipic acid dihydrazide, sebacic acid dihydrazide and adipic acid dihydrazide, or a combination of dicyandiamide, sebacic acid dihydrazide and adipic acid dihydrazide.

[0082] The curing agent is preferably dicyandiamide.

[0083] Preferably, the curing accelerator is an organic urea accelerator, preferably HUA5050 and / or HUA5200.

[0084] In the present invention, the curing accelerator is, for example, HUA5050, HUA5200, or a combination of HUA5050 and HUA5200.

[0085] Preferably, the particle size of the wollastonite powder is 10-20 μm, for example, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm.

[0086] Preferably, the particle size of the wollastonite powder is 15 μm.

[0087] Preferably, the wollastonite powder is GY-800 produced by Guangyuan Chemical.

[0088] In a preferred embodiment of the present invention, the viscosity of the epoxy toughening agent is 2000-4500 mPa·s.

[0089] In the present invention, the viscosity of the epoxy toughening agent is, for example, 2000, 2200, 2500, 2700, 3000, 3200, 3500, 3700, 4000, 4200 or 4500 mPa·s.

[0090] Preferably, the epoxy toughening agent is Dow FORTEGRA 100 and / or Yike FORTEGRA 100.

[0091] In the present invention, the epoxy toughening agent is, for example, Dow FORTEGRA 100, Yike FORTEGRA 100, or a combination of Dow FORTEGRA 100 and Yike FORTEGRA 100.

[0092] Preferably, the moisture absorbent is calcium oxide.

[0093] Preferably, the thixotropic agent includes one or more of nano calcium carbonate, organic bentonite or kaolin.

[0094] In the present invention, the thixotropic agent is, for example, nano calcium carbonate, organic bentonite, kaolin, nano calcium carbonate and organic bentonite, nano calcium carbonate and kaolin, organic bentonite and kaolin, or a combination of nano calcium carbonate, organic bentonite and kaolin.

[0095] The thixotropic agent is preferably nano-calcium carbonate, and more preferably nano-calcium carbonate having a particle size of less than 100 nm, such as 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.

[0096] Preferably, the carbon black is conductive carbon black. The use of conductive carbon black can, firstly, improve thixotropy; secondly, have a certain reinforcing effect on the cured epoxy resin system; thirdly, improve the conductivity of the cured epoxy resin system and play an anti-static role.

[0097] The conductive carbon black is preferably FB50 conductive carbon black.

[0098] In a preferred embodiment of the present invention, the particle size of the glass microspheres is 150-200 μm.

[0099] In the present invention, the particle size of the glass microbeads is, for example, 150 μm, 155 μm, 160 μm, 165 μm, 170 μm, 175 μm, 180 μm, 185 μm, 190 μm, 195 μm or 200 μm.

[0100] Preferably, the flame retardant includes one or more of aluminum hydroxide, ammonium polyphosphate or red phosphorus flame retardant.

[0101] In the present invention, the flame retardant is, for example, aluminum hydroxide, ammonium polyphosphate, red phosphorus flame retardant, aluminum hydroxide and ammonium polyphosphate, aluminum hydroxide and red phosphorus flame retardant, ammonium polyphosphate and red phosphorus flame retardant, or a combination of aluminum hydroxide, ammonium polyphosphate and red phosphorus flame retardant.

[0102] The flame retardant is preferably aluminum hydroxide.

[0103] According to a second aspect of the present invention, a method for preparing an automotive hemming adhesive is provided, the method comprising: firstly modifying bisphenol A epoxy resin with polyethersulfone, and then uniformly mixing the polyethersulfone-modified bisphenol A epoxy resin with polyurethane-modified epoxy resin, polyether-modified epoxy resin, curing agent, curing accelerator, epoxy toughening agent, carbon black, thixotropic agent, hygroscopic agent, wollastonite powder, glass microbeads and flame retardant.

[0104] Preferably, the preparation method of the polyethersulfone-modified bisphenol A epoxy resin comprises: heating the bisphenol A epoxy resin to 70-90° C., adding polyethersulfone at least three times, stirring for 40-90 minutes after each addition of polyethersulfone, and cooling when the epoxy resin becomes a uniform and transparent state.

[0105] In the present invention, the heating temperature is, for example, 70°C, 72°C, 74°C, 75°C, 76°C, 78°C, 80°C, 82°C, 84°C, 85°C, 86°C, 88°C or 90°C.

[0106] The stirring time is, for example, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min or 90 min.

[0107] Preferably, the preparation method of the automotive hemming adhesive comprises: mixing wollastonite powder, flame retardant, carbon black and polyethersulfone-modified bisphenol A epoxy resin, and stirring for 20 to 60 minutes; adding thixotropic agent, hygroscopic agent, curing agent, curing accelerator, polyurethane-modified epoxy resin and polyether-modified epoxy resin, and stirring for 20 to 60 minutes; adding glass microbeads and epoxy toughening agent, scraping the wall several times and stirring until there are no powder particles; vacuuming, stirring and degassing for 40 to 90 minutes.

[0108] In the present invention, the stirring time is, for example, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0109] The vacuum stirring and degassing time is, for example, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min or 90 min.

[0110] Preferably, the preparation method of the automotive hemming adhesive is:

[0111] First, polyethersulfone was used to modify bisphenol A epoxy resin. The bisphenol A epoxy resin was stirred and heated to 80°C, and polyethersulfone was added three times on average, each time stirring for 60 minutes to allow the polyethersulfone to be fully dispersed so that it could be more easily dissolved in the epoxy resin. When the epoxy resin became uniform and transparent, it was cooled.

[0112] Then, wollastonite powder, flame retardant, carbon black and polyethersulfone modified epoxy resin are mixed and stirred for 30 minutes; thixotropic agent, hygroscopic agent, curing agent, curing accelerator, polyurethane modified epoxy resin and polyether modified epoxy resin are added and stirred for 30 minutes; glass beads and epoxy toughening agent are added, and the wall is scraped and stirred several times until there are no powder particles; the vacuum pressure is maintained at ≥-0.08Mpa and vacuum is stirred and degassed for 60 minutes.

[0113] According to a third aspect of the present invention, there is provided an application of automotive hemming adhesive as automotive sealant.

[0114] Preferably, the automotive hemming adhesive is used for hemming areas such as vehicle doors, engine hoods or trunk lids.

[0115] Example

[0116] The present application is further described in detail below in conjunction with the embodiments. It is to be understood that the specific embodiments described herein are only used to explain the related inventions, rather than to limit the invention. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.

[0117] In the following examples, unless otherwise specified, all raw materials are commercially available products.

[0118] raw material

[0119] Bisphenol A epoxy resin: E-51

[0120] Polyurethane modified epoxy resin: EPU133L from Hahe High-Tech

[0121] Polyether modified epoxy resin: EP-1307 from Luhe High-Tech

[0122] Polyethersulfone: Solvay 3000P from the United States

[0123] Curing agent: dicyandiamide

[0124] Curing accelerator: Complex High-Tech HUA5050

[0125] Epoxy toughening agent: Dow FORTEGRA 100

[0126] Carbon black: Conductive carbon black FB50

[0127] Thixotropic agent: nano calcium carbonate

[0128] Desiccant: Calcium oxide

[0129] Wollastonite powder: Guangyuan Chemical GY-800

[0130] Flame retardant: aluminum hydroxide

[0131] The raw material ratios of Examples 1 to 7 and Comparative Examples 1 to 8 are shown in Tables 1 and 2.

[0132] Table 1 Ratios of raw materials in Examples 1 to 7

[0133]

[0134] Table 2 Ratios of raw materials in comparative examples 1 to 8

[0135]

[0136] Preparation method:

[0137] 1. Add bisphenol A epoxy resin into a stirring kettle and heat to 80°C while stirring. Add polyethersulfone into the stirring kettle three times on average and stir for 60 minutes each time to make the polyethersulfone fully dispersed and more easily dissolved in the epoxy resin. When the epoxy resin becomes uniform and transparent, cool it for use.

[0138] 2. Add wollastonite powder, flame retardant, carbon black and polyethersulfone-modified epoxy resin into a planetary mixer and stir for 30 minutes.

[0139] 3. Add thixotropic agent, hygroscopic agent, curing agent, curing accelerator, polyurethane modified epoxy resin and polyether modified epoxy resin into the planetary mixer and stir for 30 minutes;

[0140] 4. Add glass beads and epoxy toughening agent, scrape the wall several times and stir until there are no powder particles;

[0141] 5. Maintain the vacuum pressure ≥-0.08Mpa, vacuum, stir and degas for 60 minutes, and then discharge the material.

[0142] The hemming adhesives obtained in the examples and comparative examples were tested for specific gravity, liquid resistance, shear strength, T peel strength, and impact peel strength.

[0143] Specific gravity: Tested in accordance with QC / T 852-2011.

[0144] Shear Strength:

[0145] Use a steel plate with a size of 100mm×25mm×1.6mm, wipe the surface clean, apply the hemming glue on the test piece, the coating area is 25mm×12.5mm, then overlap and superimpose another same test piece with it, clamp both sides, bake it for 20 minutes under the specified conditions, place it in a standard environment for 24 hours, and then use a universal testing machine to test it at a tensile speed of 50mm / min.

[0146] T peel strength:

[0147] Use a steel plate with a size of 200mm×25mm×0.8mm, wipe the surface clean, apply the hemming glue on the test piece, the coating area is 25mm×150mm, then align and close another same test piece with it, clamp both sides, bake it for 20 minutes under the specified conditions, place it in a standard environment for 24 hours, and use a universal testing machine to test it at a tensile speed of 100mm / min.

[0148] Liquid resistance test:

[0149] On a test piece with a size of 100×25×0.8mm, apply the folding glue into a strip with a diameter of 3mm and a length of 50mm. Pour the degreasing solution, phosphating solution and electrophoresis solution into 3 clean beakers respectively, raise the temperature to 45°C, and soak the prepared test pieces in the degreasing solution, phosphating solution and electrophoresis solution for 120min respectively. Take out and check whether the surface of the strip is dissolved and whether the liquid becomes turbid.

[0150] Impact peel strength

[0151] According to the method specified in GB / T 36877-2018, a plate with a thickness of 1.6 mm and a width of 20 mm was used to prepare the sample. The hemming glue was applied on the test piece with a coating area of ​​20 mm × 30 mm. Another similar test piece was aligned and closed with it, clamped on both sides, and baked for 20 minutes under the specified conditions. After being placed in a standard environment for 24 hours, it was tested using a drop hammer impact tester.

[0152] The test results of the embodiments and comparative examples are shown in Table 3 and Table 4:

[0153] Table 3 Test results of Examples 1 to 7

[0154]

[0155] Table 4 Comparative Examples 1 to 8 Test Results

[0156]

[0157]

[0158] As shown in Tables 3 and 4, Comparative Example 1 does not use wollastonite powder, and all heavy calcium carbonate is used as filler. The obtained hemming glue has moderate dissolution and phosphating liquid slag phenomenon, and the shear impact peel strength is only 25N / mm. Comparative Example 6 uses 13 parts of calcium carbonate and 15 parts of wollastonite powder, and Comparative Example 7 uses 32 parts of wollastonite powder and 5 parts of calcium carbonate. The obtained hemming glue has slight dissolution and phosphating liquid slag phenomenon, and the impact peel strength is also low. While Examples 1-7 only use wollastonite powder, there is no dissolution and slag phenomenon, and the impact peel strength is also high, indicating that the use of wollastonite powder instead of calcium carbonate can solve the technical problems of dissolution and slag, and enhance the mechanical properties of the hemming glue to a certain extent, and have a certain positive promotion effect on the improvement of shear strength, T peel strength and impact peel strength.

[0159] As shown in Table 4, Comparative Example 2 does not use polyethersulfone modified bisphenol A epoxy resin, so the toughness of Comparative Example 2 is poor, resulting in an impact peel strength of only 15N / mm. Comparative Examples 3 and 4 have poor synergy in the dosage of each component, so their shear strength, T peeling performance and impact peeling performance are all poor. Comparative Example 5 does not use polyether modified epoxy resin, and its impact peeling strength is only 16N / mm. Comparative Example 8 has a large amount of curing agent and curing accelerator added, and the shear strength, T peeling strength and impact peeling strength are all poor, indicating that the curing reaction is too fast, and the semi-interpenetrating network crosslinking density of polyethersulfone and epoxy resin is uneven, resulting in poor toughness and impact resistance of the hemming glue.

[0160] The test results show that the hemming adhesive of the present invention has significantly improved liquid resistance and impact peel strength compared with traditional automobile hemming adhesives, and has excellent comprehensive mechanical properties.

[0161] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A hem glue for automobile, characterized in that: The invention comprises the following raw materials in parts by weight: 40 to 50 parts of epoxy resin, 2 to 5 parts of polyethersulfone, 2 to 5 parts of curing agent, 0.5 to 1.5 parts of curing accelerator, 1.5 to 5 parts of epoxy toughening agent, 3 to 5 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 5 parts of moisture absorbent, 20 to 30 parts of wollastonite powder, 3 to 5 parts of glass microspheres, and 5 to 10 parts of flame retardant; The epoxy resin comprises 20-30 parts of bisphenol A epoxy resin, 15-20 parts of polyurethane modified epoxy resin, and 3-5 parts of polyether modified epoxy resin; In the process of preparing the automotive hemming adhesive, the bisphenol A epoxy resin is firstly modified by using the polyethersulfone.

2. The automotive hem glue according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 22 to 26 parts of bisphenol A epoxy resin, 15 to 18 parts of polyurethane modified epoxy resin, 3 to 4 parts of polyether modified epoxy resin, 2 to 4 parts of polyether sulfone, 3 to 4.5 parts of curing agent, 0.5 to 1 part of curing accelerator, 2 to 2.5 parts of epoxy toughening agent, 3 to 4 parts of carbon black, 3 to 5 parts of thixotropic agent, 3 to 4 parts of hygroscopic agent, 23 to 27 parts of wollastonite powder, 3 to 3.5 parts of glass microspheres, and 6 to 8 parts of flame retardant.

3. The automotive hem glue according to claim 1, characterized in that: The bisphenol A epoxy resin is a liquid bisphenol A epoxy resin.

4. The automotive hem glue according to claim 3, characterized in that: The bisphenol A epoxy resin has a viscosity of 11000 to 40000 mPa·s and an epoxy equivalent of 180 to 250 g / eq.

5. The automotive hem glue according to claim 4, characterized in that: The bisphenol A epoxy resin is one or more of E44, E51 or YD128.

6. The automotive hem glue according to claim 3, characterized in that: The viscosity of the polyurethane modified epoxy resin is 13000-23000 mPa·s, and the epoxy equivalent is 230-260 g / eq.

7. The automotive hem glue according to claim 6, characterized in that: The polyurethane modified epoxy resin is complex high-tech EPU133L.

8. The automotive hem glue according to claim 3, characterized in that: The viscosity of the polyether-modified epoxy resin is 20000-30000 mPa·s, and the epoxy equivalent is 600-700 g / eq.

9. The automotive hem glue according to claim 8, characterized in that: The viscosity of the polyether-modified epoxy resin is 25000 mPa·s, and the epoxy equivalent is 630 g / eq.

10. The automotive hem glue according to claim 3, characterized in that: The polyether modified epoxy resin is complex high-tech EP-1307.

11. The automotive hem glue according to claim 1, characterized in that: The polyethersulfone is an ultrafine powder of 80 to 500 mesh; The curing agent includes one or more of dicyandiamide, sebacic acid dihydrazide or adipic acid dihydrazide; The curing accelerator is an organic urea accelerator; The particle size of the wollastonite powder is 10-20 μm.

12. The automotive hem glue according to claim 11, characterized in that: The polyethersulfone is Solvay 3000P from the United States; The curing agent is dicyandiamide; The curing accelerator is complex high-tech HUA5050 and / or complex high-tech HUA5200; The particle size of the wollastonite powder is 15 μm.

13. The automotive hem glue according to claim 12, characterized in that: The wollastonite powder is GY-800 produced by Guangyuan Chemical.

14. The automotive hem glue according to claim 1, characterized in that: The viscosity of the epoxy toughening agent is 2000-4500 mPa·s; The desiccant is calcium oxide; The thixotropic agent includes one or more of nano calcium carbonate, organic bentonite or kaolin; The carbon black is conductive carbon black.

15. The automotive hem glue according to claim 14, characterized in that: The epoxy toughening agent is Dow FORTEGRA100 and / or Yike FORTEGRA100; The thixotropic agent is nano calcium carbonate.

16. The automotive hem glue according to claim 15, characterized in that: The thixotropic agent is nano calcium carbonate with a particle size less than 100 nm.

17. The automotive hem glue according to claim 1, characterized in that: The particle size of the glass microspheres is 150 to 200 μm; The flame retardant includes one or more of aluminum hydroxide, ammonium polyphosphate or red phosphorus flame retardant.

18. The automotive hem glue according to claim 17, characterized in that: The flame retardant is aluminum hydroxide.

19. The method for preparing the automotive hemming adhesive according to any one of claims 1 to 18, characterized in that: Firstly, bisphenol A epoxy resin is modified by using polyethersulfone, and then the polyethersulfone-modified bisphenol A epoxy resin is mixed with polyurethane-modified epoxy resin, polyether-modified epoxy resin, curing agent, curing accelerator, epoxy toughening agent, carbon black, thixotropic agent, hygroscopic agent, wollastonite powder, glass microspheres and flame retardant.

20. The method for preparing the automotive hem glue according to claim 7, characterized in that: The preparation method of polyethersulfone-modified bisphenol A epoxy resin comprises: heating bisphenol A epoxy resin to 70-90°C, adding polyethersulfone at least three times, stirring for 40-90 minutes after each addition of polyethersulfone, and cooling when the epoxy resin becomes uniform and transparent.

21. The method for preparing the automotive hem glue according to claim 20, characterized in that: The preparation method of automotive hemming adhesive includes: mixing wollastonite powder, flame retardant, carbon black and polyethersulfone modified bisphenol A epoxy resin, stirring for 20 to 60 minutes; adding thixotropic agent, hygroscopic agent, curing agent, curing accelerator, polyurethane modified epoxy resin and polyether modified epoxy resin, stirring for 20 to 60 minutes; adding glass microbeads and epoxy toughening agent, scraping the wall for multiple times and stirring until there are no powder particles; vacuuming, stirring and degassing for 40 to 90 minutes.

22. Use of the automotive hemming adhesive as claimed in any one of claims 1 to 18 as automotive sealant.

23. The use of the automotive hem glue according to claim 22, characterized in that: The automobile hemming adhesive is used for the hemming parts of vehicle doors, engine hoods or luggage trunk lids.