A method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction
By using sodium fluoride and anhydrous magnesium chloride as additives in the thermite reduction process, the problem of high impurity content in magnesia-aluminum spinel during magnesite smelting of low-grade magnesite is solved, and high-purity purification of magnesite-aluminum spinel is achieved. , improving the economy and feasibility of magnesium refining.
Patent Information
- Application Number
- CN202310018609.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-06
AI Technical Summary
When low-grade magnesite is used as raw material for magnesium smelting, the impurity content of magnesia-aluminum spinel is high, making it difficult to meet national standards, which affects the economy and feasibility of the technology.
During the thermite reduction process, sodium fluoride and anhydrous magnesium chloride are added as additives to react the impurities with magnesium oxide to form easily distillable substances, and the magnesia-aluminum spinel is further purified through vacuum reduction and alkali dissolution reactions.
The purity of magnesite-aluminum spinel is significantly improved, and the economy and feasibility of magnesite-making by thermite reduction of low-grade magnesite are enhanced.
Smart Images

Figure CN116005007B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium smelting, and more specifically to a method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction. Background Art
[0002] At present, more than 85% of magnesium in the world is produced by the Pidgeon process. The Pidgeon process is a method of vacuum silicon thermal reduction of magnesium using dolomite as raw material and ferrosilicon as reducing agent. This method has high energy consumption, large material consumption, high carbon emissions, and the reduction slag cannot be used to produce magnesium. These shortcomings have seriously affected the sustainable development of the magnesium industry. Therefore, it is urgent to develop a new magnesium smelting technology with low energy consumption, low carbon emissions and no waste slag emissions.
[0003] Patent CN101942573B proposes a method for preparing magnesium metal with active magnesium oxide and aluminum or aluminum alloy as raw materials and preparing magnesium aluminate spinel as a byproduct. The method uses magnesite or brucite to calcine magnesium oxide, and then uses aluminum or aluminum alloy as a reducing agent to perform vacuum thermal reduction to smelt magnesium. After reduction, magnesium metal and a reduction slag whose main component is magnesium aluminate spinel are obtained. After high-temperature calcination of the reduction slag, a high-density magnesium aluminate spinel refractory material is obtained. The method of this patent can reduce the energy consumption of the magnesium smelting process by more than 50% compared with the Pidgeon method, reduce the raw material consumption by more than 50%, reduce carbon emissions by 60%, and the reduction slag can be fully utilized.
[0004] The above patented method is used for magnesium smelting, which has low energy consumption and low carbon emissions. The reduced slag can be used to prepare magnesia-alumina spinel refractory materials. It is a promising new magnesium smelting technology. However, due to the exhaustion of high-quality magnesite in my country, the currently mined magnesite has a high impurity content (mainly high silicon dioxide and calcium oxide content). In the process of producing metallic magnesium using the method of patent CN101942573B, all impurities in the reduced material magnesite are left in the reduced slag, resulting in a high impurity content in the reduced slag, which in turn makes the magnesia-alumina spinel produced with the reduced slag as raw material have a high impurity content, especially the calcium oxide and silicon dioxide content are both above 1%, which is difficult to meet the national standard for magnesia-alumina spinel, seriously reducing the economy and feasibility of the technology. Summary of the invention
[0005] To this end, the technical problem to be solved by the present invention is to provide a method for preparing metallic magnesium and magnesia-alumina spinel by aluminothermic reduction, so as to solve the problem that when low-quality dolomite ore is used as raw material for magnesium smelting, the by-product magnesia-alumina spinel has a high impurity content and is difficult to meet the national standards for magnesia-alumina spinel.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, comprising the following steps:
[0008] Step (1), calcining and grinding low-grade magnesite to obtain magnesium oxide powder;
[0009] Step (2), using aluminum powder as a reducing agent, sodium fluoride and anhydrous magnesium chloride as additives, and uniformly mixing magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride to obtain a mixed material;
[0010] Step (3), pressing the mixture into agglomerates at room temperature;
[0011] Step (4), placing the agglomerate in a vacuum reduction tank and performing a reduction reaction under vacuum conditions; after the reduction reaction is completed, a reduction slag is obtained in the reduction zone, and a crystallizer is collected to obtain a crystallized mixture;
[0012] Step (5), placing the reduced residue in a sodium hydroxide solution for dissolution reaction, and filtering after the dissolution reaction is completed to obtain a filter residue;
[0013] Step (6), calcining the filter residue to obtain magnesium-aluminum spinel after calcination;
[0014] Step (7), placing the crystal mixture in a refining furnace for refining, and obtaining magnesium liquid and refined slag after the refining is completed. The present invention uses low-grade magnesite as raw material, aluminum as a reducing agent, sodium fluoride and magnesium chloride as additives to prepare metallic magnesium, and uses magnesium smelting reduction slag as raw material to prepare magnesia-alumina spinel; its basic principle is to add additives during the reduction process, so that the additives react with impurities in the low-grade magnesite, convert them into distillable substances for removal, and achieve the purpose of purifying magnesia-alumina spinel.
[0015] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (1), the calcination temperature of magnesite is 800-1100° C., and the calcination time is 0.5-4 hours. If the calcination temperature of magnesite is too low or the calcination time is too short, the calcination decomposition of magnesite will not be complete. If the calcination temperature is too high or the calcination time is too long, the activity of magnesium oxide obtained by calcination will be reduced. By controlling the calcination temperature of magnesite to 800-1100° C. and the calcination time to 0.5-4 hours, it is possible to ensure that magnesite is fully decomposed and magnesium oxide with higher activity is obtained.
[0016] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (2), the mass ratio of magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride is (2.0-5.0):1:(0.03-0.20):(0.03-0.20); under this ratio, the reduction reaction efficiency is high and the impurity removal effect is good.
[0017] The above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (1), the particle size of the magnesium oxide powder is less than or equal to 0.15 mm; in step (2), the particle size of the mixed material is less than or equal to 0.15 mm; if the particle size of the raw material particles is too large, the reduction rate of the magnesium oxide will be reduced.
[0018] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (3), the pressing pressure is 100-200 MPa; if the pressing pressure is too high, the reduction rate of magnesium oxide will be affected.
[0019] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (4), the absolute pressure under vacuum conditions is 0.01-30 Pa. If the absolute pressure is too high, it will affect the reduction rate of magnesium oxide. The temperature of the reduction reaction is 1100-1300°C, and the reaction time is 9-16 hours. During the reduction process, magnesium oxide is reduced by aluminum to gaseous metallic magnesium, which moves to the crystallization zone and crystallizes on the crystallizer, and the reduction slag remains in the reduction zone. According to the different proportions of magnesium oxide and aluminum powder, the main component of the reduction slag is MgO·Al 2 O 3 +MgO or MgO·Al 2 O 3 +Al 2 O 3 .
[0020] In the reduction reaction process of the present invention, in addition to the reduction reaction of magnesium oxide, the additives NaF and MgCl 2 A series of reactions will also occur. Through these reactions, the reduction reaction can be accelerated, and most of the impurities CaO and SiO in the reduction slag can be reduced to 2 Remove, to achieve the purpose of improving magnesium reduction rate and purifying reduction slag. Additives NaF and MgCl 2 The main reactions that occur are shown in equations 1-6. Through these reactions, most of the CaO impurities in the magnesium oxide powder are converted into CaCl 2 It is vacuum distilled and crystallized in a crystallizer, and the SiO 2 Impurities are partially converted into SiF 4 Gas removal. Residual additive MgCl during reduction 2 and NaF, and react to form other components (metallic sodium and Na 3 AlF 6 ) is also vacuum distilled and crystallized in a crystallizer.
[0021] MgCl 2 +CaO=CaCl 2 +MgO(1)
[0022] Al+6NaF=3Na+Na 3 AlF 6 (2)
[0023] SiO 2 +4NaF=2Na 2 O+SiF 4 (3)
[0024] 3SiO 2 +2Na 3 AlF 6 =3Na 2 O+Al 2 O 3 +3SiF 4 (4)
[0025] 2Na+MgO=Na 2 O+Mg(5)
[0026] 3Na 2 O+2Al=6Na+Al 2 O 3 (6)
[0027] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (5), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 1 to 10 wt%; the mass ratio of the sodium hydroxide solution to the reduction slag is (2 to 10):1, and the reduction slag obtained after reduction exists in the form of porous agglomerates; the temperature of the dissolution reaction is 10 to 80°C, and the dissolution reaction time is 0.5 to 2 hours. Under the dissolution reaction conditions, a relatively ideal dissolution effect can be obtained. During the dissolution process, the unreacted metallic aluminum powder and part of the SiO 2 It reacts with NaOH solution to convert into sodium aluminate and sodium silicate, which enter into the dissolution solution and are separated from the slag (as shown in equations 7 and 8):
[0028] SiO 2 +2NaOH=Na 2 SiO 3 +H 2 O (7)
[0029] 2Al+2NaOH+6H 2 O=2NaAl(OH) 4 +3H 2 (8).
[0030] In the above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, in step (6), the calcination temperature is 1700-1800°C, and the calcination time is 12-36h. If the calcination temperature is lower than 1700°C, the density of the obtained magnesium-aluminum spinel is unqualified, but if it is higher than 1800°C, the spinel will melt; if the calcination time is lower than 12h, the density of the obtained magnesium-aluminum spinel will also be unqualified; if the calcination time is higher than 36h, the unit consumption of the product will increase and the cost will be increased; after calcination, a high-purity density of 3.25-3.35g / cm 3 The magnesium aluminum spinel refractory product; in step (7), the refining temperature is 700-750°C, and the refining time is 0.5-2h; during refining, if the refining temperature is too low or the refining time is insufficient, the impurity content after refining will be high due to the high viscosity of the magnesium liquid, but if the refining temperature is too high or the refining time is too long, the magnesium combustion loss will be serious and the magnesium yield will be reduced. During the reduction process, the metal magnesium and the additive MgCl remaining in the material 2 and NaF, and react to form metallic sodium, CaCl 2 and Na 3 AlF 6 The above-mentioned materials are all crystallized on the crystallizer. These crystal mixtures are taken out from the crystallizer and put into the refining furnace for refining. The refining process obtains magnesium liquid and refining slag.
[0031] The above-mentioned method for preparing metallic magnesium and magnesia-aluminum spinel by aluminothermic reduction is realized by utilizing a production system for preparing metallic magnesium and magnesia-aluminum spinel by aluminothermic reduction; the production system for preparing metallic magnesium and magnesia-aluminum spinel by aluminothermic reduction comprises a magnesium oxide production mechanism, a mixing mechanism, a molding mechanism, a reduction mechanism, a metallic magnesium generation mechanism and a magnesia-aluminum spinel generation mechanism; the magnesium oxide discharge port of the magnesium oxide production mechanism is connected with the magnesium oxide feed port of the mixing mechanism; the discharge port of the mixing mechanism is connected with the feed port of the molding mechanism; the discharge port of the molding mechanism is adjacent to the feed port of the reduction mechanism; the crystallized material discharge port of the reduction mechanism is connected with the feed port of the metallic magnesium generation mechanism; the reduction slag discharge port of the reduction mechanism is adjacent to the feed port of the magnesia-aluminum spinel generation mechanism.
[0032] The above-mentioned method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, the magnesium oxide production mechanism comprises a crusher, a first calcining furnace and a pulverizer; the discharge port of the crusher is connected to the feed port of the first calcining furnace through a first conveyor belt; the discharge port of the first calcining furnace is connected to the feed port of the pulverizer through a second conveyor belt;
[0033] The mixing mechanism includes a feeder and a mixer; the feed outlet of the feeder is located directly above the additive feed outlet of the mixer; the magnesium oxide feed outlet of the pulverizer is connected to the magnesium oxide feed outlet of the mixer through a third conveyor belt;
[0034] The molding mechanism is a powder molding machine; the discharge port of the mixer is connected to the feed port of the powder molding machine through a fourth conveyor belt;
[0035] The reduction mechanism is a vacuum reduction tank, which has a crystallization zone and a reduction slag zone; the powder forming machine conveys the formed agglomerates to a feed port adjacent to the vacuum reduction tank through a fifth conveyor belt;
[0036] The magnesium metal generating mechanism comprises a refining furnace; the crystallized material discharge port of the crystallization zone is connected to the feed port of the refining furnace through a seventh conveyor belt;
[0037] The magnesium-aluminum spinel generating mechanism includes a molten pool, a filter and a second calcining furnace; the fluid outlet end of the molten pool is fluidly connected to the fluid inlet end of the filter through a pipeline; the filter residue outlet end of the filter is connected to the feed port of the second calcining furnace through an eighth conveyor belt; the reduced slag discharge port of the reduced slag zone conveys the reduced slag to the feed port adjacent to the molten pool through a sixth conveyor belt.
[0038] The reduction tank used in the reduction process of the present invention is the same as the reduction tank of the current Pidgeon process for magnesium smelting; the refining process of the crystallized product is the same as the current Pidgeon process for magnesium smelting; the main composition of the magnesium-aluminum spinel product is related to the proportion of magnesium oxide and aluminum powder. By adjusting the ratio of magnesium oxide powder to aluminum powder in the batching process, various magnesium-aluminum spinel refractory materials containing 0 to 95 wt% of aluminum oxide can be produced.
[0039] The technical solution of the present invention achieves the following beneficial technical effects:
[0040] The present invention adds sodium fluoride and magnesium chloride as additives in the aluminothermic reduction magnesium smelting process of low-grade magnesite to reduce the main impurities CaO and SiO 2 It reacts with additives to generate easily distillable substances which are removed. In addition, the reduction slag is further purified by leaching with alkaline solution, so that the purity of the prepared magnesia-alumina spinel is greatly improved, thereby improving the economy and feasibility of aluminothermic reduction of low-grade magnesia. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A schematic diagram of a process flow of a method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction in an embodiment of the present invention;
[0042] Figure 2 A schematic structural diagram of a production system for preparing metallic magnesium and magnesium-aluminum spinel using aluminothermic reduction in Example 2 of the present invention.
[0043] The reference numerals in the figure are as follows: 1-crusher; 2-first calcining furnace; 3-pulverizer; 4-feeder; 5-mixer; 6-powder forming machine; 7-vacuum reduction tank; 8-melting tank; 9-filter; 10-second calcining furnace; 11-first conveyor belt; 12-second conveyor belt; 13-third conveyor belt; 14-fourth conveyor belt; 15-fifth conveyor belt; 16-sixth conveyor belt; 17-seventh conveyor belt; 18-eighth conveyor belt; 19-pipeline; 20-refining furnace; 71-crystallization zone; 72-reduction slag zone; 81-sodium hydroxide solution. DETAILED DESCRIPTION
[0044] Example 1
[0045] In this embodiment, the process flow of the method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction is as follows: Figure 1 As shown; specifically includes the following steps:
[0046] Step (1), calcining low-grade magnesite at 1000° C. for 2 h and then grinding it to a particle size less than or equal to 0.15 mm to obtain magnesium oxide powder; in this embodiment, the impurity content in the low-grade magnesite is relatively high, the content of silicon dioxide is 1.00wt%, and the content of calcium oxide is 1.30wt%.
[0047] Step (2), using aluminum powder with a particle size less than or equal to 0.15 mm as a reducing agent, sodium fluoride and anhydrous magnesium chloride with a particle size less than or equal to 0.15 mm as additives, and mixing magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride in a mass ratio of 3:1:0.1:0.1 to obtain a mixed material;
[0048] Step (3), pressing the mixed material into agglomerates at 150 MPa and room temperature;
[0049] Step (4), placing the agglomerate in a vacuum reduction tank, and performing a reduction reaction under vacuum conditions. In this embodiment, the absolute pressure in the vacuum reduction tank is 10Pa; the temperature of the reduction reaction is 1200°C, and the reaction time is 12h. In other embodiments, the temperature of the reduction reaction can be selected at any temperature between 1100 and 1300°C, and the reaction time can be selected at any time between 9 and 16h. Under this reaction condition, the reduction effect of magnesium oxide is good and the production cost is low. After the reduction reaction is completed, a reduction slag is obtained in the reduction zone, and the crystallized mixture is collected in a crystallizer;
[0050] Step (5), placing the reduced slag in a sodium hydroxide solution with a mass fraction of 5wt% for dissolution reaction, the mass ratio of the sodium hydroxide solution to the reduced slag is 8:1; the temperature of the dissolution reaction is 25°C, and the dissolution reaction time is 1h; after the dissolution reaction is completed, filtering is performed to obtain a filter residue; of course, in other embodiments, the mass ratio of the sodium hydroxide solution to the reduced slag can be selected from any value between (2 and 10):1, which can give full play to the dissolution effect of sodium hydroxide, so that the metallic aluminum powder and part of SiO in the reduced slag are removed. 2 Fully react with NaOH solution; the mass fraction of the sodium hydroxide solution can be selected to be any concentration between 1 and 10wt%, and the use of sodium hydroxide solutions within this concentration range has a good dissolution effect and will not cause serious corrosion to the equipment.
[0051] Step (6), calcining the filter residue at 1700°C for 24 hours, and obtaining magnesium-aluminum spinel after calcination. The density of magnesium-aluminum spinel prepared in this embodiment is 3.30 g / cm 3 ; The calcium oxide content in the magnesium aluminum spinel is 0.15wt%, and the silicon dioxide content is 0.10wt%.
[0052] Step (7), placing the crystallized mixture in a refining furnace for refining at a refining temperature of 720° C. for a refining time of 1.5 h; after the refining is completed, magnesium liquid and refining slag are obtained, and the magnesium liquid is cast to obtain a metal magnesium ingot.
[0053] Example 2
[0054] This embodiment uses a production system for preparing metallic magnesium and magnesia-alumina spinel by aluminothermic reduction to achieve the preparation of metallic magnesium and magnesia-alumina spinel by aluminothermic reduction; the production system is as follows; Figure 2 shown; from Figure 2 It can be seen that the production system of this embodiment includes a magnesium oxide production mechanism, a mixing mechanism, a molding mechanism, a reduction mechanism, a metal magnesium generation mechanism and a magnesium-aluminum spinel generation mechanism; the magnesium oxide production mechanism includes a crusher 1, a first calcining furnace 2 and a pulverizer 3; the mixing mechanism includes a feeder 4 and a mixer 5; the molding mechanism is a powder molding machine 6; the reduction mechanism is a vacuum reduction tank 7, and the vacuum reduction tank 7 has a crystallization area 71 and a reduction slag area 72; the metal magnesium generation mechanism includes a refining furnace 20; in some other embodiments, the metal magnesium generation mechanism also includes a magnesium liquid casting device, and the fluid outlet of the refining furnace 20 is fluidly connected to the fluid inlet of the magnesium liquid casting device; the magnesium-aluminum spinel generation mechanism includes a melting pool 8, a filter 9 and a second calcining furnace 10.
[0055] The discharge port of the crusher 1 is connected to the feed port of the first calcining furnace 2 through the first conveyor belt 11; the discharge port of the first calcining furnace 2 is connected to the feed port of the pulverizer 3 through the second conveyor belt 12; the discharge port of the pulverizer 3 is connected to the magnesium oxide feed port of the mixer 5 through the third conveyor belt 13; the discharge port of the feeder 4 is located directly above the additive feed port of the mixer 5; the discharge port of the mixer 5 is connected to the feed port of the powder forming machine 6 through the fourth conveyor belt 14; the powder forming machine 6 conveys the formed agglomerates to the feed port adjacent to the vacuum reduction tank 7 through the fifth conveyor belt 15;
[0056] The crystallized material outlet of the crystallization zone 71 is connected to the feed port of the refining furnace 20 through the seventh conveyor belt 17; the reduced slag outlet of the reduced slag zone 72 conveys the reduced slag to the feed port adjacent to the molten pool 8 through the sixth conveyor belt 16; the fluid outlet end of the molten pool 8 is fluidly connected to the fluid inlet end of the filter 9 through the pipeline 19; the filter residue outlet end of the filter 9 is connected to the feed port of the second calcining furnace 10 through the eighth conveyor belt 18. In this embodiment, the molten pool 8 contains a sodium hydroxide solution 81 with a mass fraction of 1 to 10wt%.
[0057] The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction in this embodiment specifically comprises the following steps:
[0058] Step (1), crushing low-grade dolomite in a crusher 1 and conveying it to a first calcining furnace 2 via a first conveyor belt 11, calcining it at 1100° C. for 1 hour in the first calcining furnace 2, and then conveying it to a pulverizer 3 via a second conveyor belt 12 and grinding it to a particle size less than or equal to 0.15 mm to obtain magnesium oxide powder; in this embodiment, the impurity content in the low-grade dolomite is relatively high, the content of silicon dioxide is 1.10wt%, and the content of calcium oxide is 1.80wt%.
[0059] Step (2), the magnesium oxide powder processed by the pulverizer 3 is conveyed to the mixer 5 via the third conveyor belt 13, and aluminum powder with a particle size less than or equal to 0.15 mm is added to the mixer 5 via the feeder 4 as a reducing agent, and sodium fluoride and anhydrous magnesium chloride with a particle size less than or equal to 0.15 mm are used as additives, and the mass ratio of magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride in the mixer 5 is controlled to be 5:1:0.2:0.2, and the mixture is uniformly mixed in the mixer 5 to obtain a mixed material;
[0060] Step (3), the mixed material is conveyed to the powder forming machine 6 via the fourth conveyor belt 14, and is pressed in the powder forming machine 6 at 200 MPa and room temperature to obtain agglomerates;
[0061] Step (4), the agglomerate is conveyed to the feed port of the adjacent vacuum reduction tank via the fifth conveyor belt 15, and the agglomerate is placed in the vacuum reduction tank 7 to perform a reduction reaction under vacuum conditions. In this embodiment, the absolute pressure in the vacuum reduction tank is maintained at 20 Pa; the temperature of the reduction reaction is 1100° C., and the reaction time is 15 h; after the reduction reaction is completed, a reduction slag is obtained in the reduction slag area 72, and a crystallization mixture is obtained by collecting in the crystallization area 71;
[0062] Step (5), the reduced slag is conveyed to the molten pool 8 by the sixth conveyor belt 16, and the reduced slag is subjected to a dissolution reaction with a sodium hydroxide solution having a mass fraction of 10 wt % in the molten pool 8, wherein the mass ratio of the sodium hydroxide solution to the reduced slag is 10:1; the dissolution reaction temperature is 40° C., and the dissolution reaction time is 0.5 h; after the dissolution reaction is completed, the reaction mixture is conveyed to a filter through a pipeline 19 for filtration to obtain a filter residue;
[0063] Step (6), the filter residue is conveyed to the second calcining furnace 10 via the eighth conveyor belt 18, and calcined at 1800°C for 14 hours, and magnesium-aluminum spinel is obtained after the calcination. The density of the magnesium-aluminum spinel prepared in this embodiment is 3.35 g / cm 3 ; The calcium oxide content in the magnesium aluminum spinel is 0.15wt%, and the silicon dioxide content is 0.20wt%.
[0064] Step (7), conveying the crystallized mixture to the refining furnace 20 via the seventh conveyor belt 17 for refining, the refining temperature is 750° C., and the refining time is 1 hour; after the refining is completed, magnesium liquid and refining slag are obtained, and the magnesium liquid is cast to obtain a metal magnesium ingot.
[0065] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction, It is characterized in that The steps include: Step (1), calcining and grinding magnesite to obtain magnesium oxide powder; Step (2), mixing magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride uniformly to obtain a mixed material; Step (3), pressing the mixture into agglomerates at room temperature; Step (4), placing the agglomerate in a vacuum reduction tank and performing a reduction reaction under vacuum conditions; after the reduction reaction is completed, a reduction slag is obtained in the reduction zone, and a crystallizer is collected to obtain a crystallized mixture; Step (5), placing the reduced residue in a sodium hydroxide solution for dissolution reaction, and filtering after the dissolution reaction is completed to obtain a filter residue; Step (6), calcining the filter residue to obtain magnesium-aluminum spinel after calcination; Step (7), placing the crystallized mixture in a refining furnace for refining, and obtaining magnesium liquid and refined slag after the refining is completed.
2. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (1), the calcination temperature of magnesite is 800-1100° C., and the calcination time is 0.5-4 h.
3. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (2), the mass ratio of magnesium oxide powder, aluminum powder, sodium fluoride and anhydrous magnesium chloride is (2.0-5.0):1:(0.03-0.20):(0.03-0.20).
4. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (1), the particle size of the magnesium oxide powder is less than or equal to 0.15 mm; in step (2), the particle size of the mixed material is less than or equal to 0.15 mm.
5. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (3), the pressing pressure is 100 to 200 MPa.
6. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (4), the absolute pressure under vacuum conditions is 0.01-30 Pa; the temperature of the reduction reaction is 1100-1300° C., and the reaction time is 9-16 h.
7. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (5), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 1-10wt%; the mass ratio of the sodium hydroxide solution to the reduction slag is (2-10):1; the temperature of the dissolution reaction is 10-80°C, and the dissolution reaction time is 0.5-2h.
8. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that In step (6), the calcination temperature is 1700-1800° C., and the calcination time is 12-36 hours; in step (7), the refining temperature is 700-750° C., and the refining time is 0.5-2 hours.
9. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 1, It is characterized in that The production system for preparing metallic magnesium and magnesia-aluminum spinel by aluminothermic reduction is realized; the production system for preparing metallic magnesium and magnesia-aluminum spinel by aluminothermic reduction comprises a magnesium oxide production mechanism, a mixing mechanism, a molding mechanism, a reduction mechanism, a metallic magnesium generation mechanism and a magnesia-aluminum spinel generation mechanism; the magnesium oxide discharge port of the magnesium oxide production mechanism is connected with the magnesium oxide feed port of the mixing mechanism; the discharge port of the mixing mechanism is connected with the feed port of the molding mechanism; the discharge port of the molding mechanism is adjacent to the feed port of the reduction mechanism; the crystallized material discharge port of the reduction mechanism is connected with the feed port of the metallic magnesium generation mechanism; the reduction slag discharge port of the reduction mechanism is adjacent to the feed port of the magnesia-aluminum spinel generation mechanism.
10. The method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction according to claim 9, It is characterized in that The magnesium oxide production mechanism comprises a crusher (1), a first calcining furnace (2) and a pulverizer (3); the discharge port of the crusher (1) is connected to the feed port of the first calcining furnace (2) via a first conveyor belt (11); the discharge port of the first calcining furnace (2) is connected to the feed port of the pulverizer (3) via a second conveyor belt (12); The mixing mechanism comprises a feeder (4) and a mixer (5); the discharge port of the feeder (4) is located directly above the additive feed port of the mixer (5); the magnesium oxide discharge port of the pulverizer (3) is connected to the magnesium oxide feed port of the mixer (5) via a third conveyor belt (13); The molding mechanism is a powder molding machine (6); the discharge port of the mixer (5) is connected to the feed port of the powder molding machine (6) via a fourth conveyor belt (14); The reduction mechanism is a vacuum reduction tank (7), and the vacuum reduction tank (7) has a crystallization area (71) and a reduction slag area (72); the powder forming machine (6) conveys the formed agglomerates to a feed port adjacent to the vacuum reduction tank (7) via a fifth conveyor belt (15); The magnesium metal generating mechanism comprises a refining furnace (20); the crystallized material outlet of the crystallization zone (71) is connected to the feed inlet of the refining furnace (20) via a seventh conveyor belt (17); The magnesium-aluminum spinel generating mechanism comprises a molten pool (8), a filter (9) and a second calcining furnace (10); the fluid outlet end of the molten pool (8) is fluidly connected to the fluid inlet end of the filter (9) via a pipeline (19); the filter residue outlet end of the filter (9) is connected to the feed port of the second calcining furnace (10) via an eighth conveyor belt (18); the reduction slag outlet of the reduction slag zone (72) conveys the reduction slag to the feed port adjacent to the molten pool (8) via a sixth conveyor belt (16).