A low-cost Q550D steel plate using V instead of Mo and its production method

By using V instead of Mo in Q550D steel plate and adopting high-temperature, low-speed large-pressure rolling, stacking and tempering heat treatment processes, the problems of high production costs and long heat treatment cycles in the existing technology are solved, and low-cost and high-quality steel plates are achieved The performance of Q550D steel plates is produced to meet or exceed the performance requirements of the Q550D standard.

CN116005081BActive Publication Date: 2024-11-22NANYANG HANYE SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211557471.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-22
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The production cost of existing Q550D steel plates is high and the heat treatment cycle is long, which leads to an increase in alloy cost and affects its promotion and application.

Method used

The composition design and heat treatment process of low-cost Q550D steel plates that replace Mo with V, reduce alloy costs and shorten production cycles by adjusting chemical composition and process flow, including high-temperature and low-speed large-pressure rolling, stack cooling and tempering heat treatment, etc. Ensure the strength and toughness of the steel plate.

Benefits of technology

The production of Q550D steel plates has been achieved with low-cost performance reaching or exceeding the same steel standards, reducing alloy cost and shortening production cycle. The yield strength, tensile strength and elongation after break of the steel plate have reached or exceeded the Q550D requirements, and at the same time, reducing welding cracks Sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003983873900000041
    Figure BDA0003983873900000041
Patent Text Reader

Abstract

The present invention belongs to the field of wide and thick plate production, and specifically relates to a low-cost Q550D steel plate using V instead of Mo and a production method thereof. The thickness of the steel plate is 50-80 mm, and includes the following chemical components (unit, wt%): C: 0.10-0.17, Si: 0.10-0.25, Mn: 1.50-1.67, P≤0.010, S≤0.005, Als: 0.020-0.050, Nb: 0.020-0.045, Cr: 0.4-0.9, V: 0.050-0.080, Ti: 0.010-0.020, B: 0.0018-0.0022, and the others are Fe and residual elements; its structure is mainly bainite, containing a small amount of martensite and ferrite. Under the premise of ensuring performance, the present invention optimizes alloy combination, shortens production cycle, reduces production cost, and has good market promotion value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wide and thick plate production, and specifically relates to a low-cost Q550D steel plate using V instead of Mo and a production method thereof. Background Art

[0002] In recent years, with the massive investment in public infrastructure in my country, the construction machinery and coal mining machinery industries have flourished. Q550D is mainly used in the production of large and medium-sized construction machinery and coal mining machinery industries. At present, steel plates with a thickness greater than 50 mm mainly use C+Mn+Nb+V+Cr+Mo components, and the heat treatment process mainly uses quenching + tempering process. The defects of this solution are high alloy cost and long heat treatment cycle, which further increases the production cost and is not conducive to promotion. Summary of the invention

[0003] To solve the above-mentioned defects, the purpose of the present invention is to provide a low-cost Q550D steel plate with V instead of Mo, replacing the composition design and heat treatment process of the conventional solution, while ensuring the performance, reducing the alloy cost, shortening the production cycle, and thereby reducing the production cost of this steel.

[0004] The object of the present invention is to provide a method for producing a low-cost Q550D steel plate by replacing Mo with V.

[0005] To achieve the above object, the present invention is implemented in the following ways:

[0006] A low-cost Q550D steel plate using V instead of Mo, the thickness of the steel plate is 50-80 mm, and the steel plate comprises the following chemical components by mass content (unit, wt%): C: 0.10-0.17, Si: 0.10-0.25, Mn: 1.50-1.67, P≤0.010, S≤0.005, Als: 0.020-0.050, Nb: 0.020-0.045, Cr: 0.4-0.9, V: 0.050-0.080, Ti: 0.010-0.020, B: 0.0018-0.0022, and the rest are Fe and residual elements;

[0007] It should be noted that molybdenum (Mo) is an alloying element that reduces the γ-Fe phase area and expands the α-Fe phase area. Molybdenum can significantly inhibit the self-diffusion of iron in iron, increase the recrystallization temperature of the solid solution, and is also a strong carbide-forming element. Molybdenum solid solution in the base metal can increase the recrystallization temperature of the solid solution. As an alloying element of steel, Mo can improve the strength of steel, especially high-temperature strength and toughness; improve the wear resistance of steel and improve hardenability, weldability and heat resistance. However, Mo is brittle at room temperature, which will lead to poor processing and weldability of steel, seriously affecting the expansion of its application field; and Mo is a precious alloy with a relatively high price. After adding Mo, the product does not have a market competitive advantage. Vanadium (V) is a difficult metal with a high melting point (1910). V is an alloying element that reduces the y-Fe phase area and expands the a-Fe phase area. It is a strong carbide-forming element. After high-temperature tempering, these strong carbides precipitate dispersed heterogeneous particles. The interaction between the precipitated particles and the moving dislocations improves the strength of the steel.

[0008] In addition, this scheme adopts a low P and low Si design. P can cause serious segregation of steel, increase temper brittleness, and reduce the plasticity and toughness of steel, which is not conducive to the subsequent welding of steel; Si can significantly increase the ductile-brittle transition temperature and reduce the welding performance of steel, so the Si content is appropriately reduced in high-strength steel, and the strength is improved by appropriately increasing the Cr content; the precipitation and strengthening of micro-alloying elements Nb, V, and Ti carbides keeps the original austenite grains refined, which is crucial to toughness, strength and weldability; B element can improve the hardenability of steel to ensure excellent strength and toughness after tempering, while relatively reducing the content of other alloying elements to ensure the welding performance of steel. The overall composition design ensures that the carbon equivalent Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15≤0.65% and the low welding crack sensitivity coefficient Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B≤0.30%.

[0009] The production method of the steel plate includes rolling, stack cooling, and tempering heat treatment, which is specifically as follows:

[0010] a. Rolling process: in the rough rolling stage, "high temperature, low speed and large reduction" rolling is adopted, the rolling start temperature is ≥1220℃, and the pass reduction is ≥85mm, so that the deformation can fully penetrate to the center in the thickness direction, effectively weld and mesh the defects such as looseness inside the ingot, fully break the original cast structure, make the steel plate grains uniform and refined, and further heal the loose defects inside the ingot to achieve the internal density of the steel plate; after the rough rolling, IC fast cooling is used to cool the intermediate billet to 840-860℃ for the second stage of finishing rolling. During the finishing rolling process, high-pressure water cooling is turned on throughout the process. Due to the fast surface temperature drop and low temperature, it is in the unrecrystallized austenite area, and the grain size basically maintains the original size. As the distance to the center area increases, the temperature increases, the recrystallization percentage continues to increase, and the average grain size decreases until the austenite is completely recrystallized. The size is relatively uniform. After the final rolling, the temperature of the steel plate is controlled at 820-840℃. After the rolling, the steel plate is relaxed on the roller for 60-80s. During the relaxation process, the high dislocation density deformed austenite gradually forms a cellular substructure of 3-5μm in size, which is equivalent to increasing the grain boundary, so that the microalloy compound is fully precipitated on the interface of the substructure. The subsequent phase transformation occurs inside the substructure. Due to the effect of the subgrain boundary, the phase transformation organization is finer, thereby obtaining bainite with shorter lath bundles and narrower laths, thereby improving the toughness and strength of the steel plate. After the relaxation is completed, the temperature of the steel plate is controlled at 800-820℃, and the steel plate enters the NCC fast cooling at a speed of 0.5m / s. The cooling rate is controlled at 8-12℃ / S, and the temperature of the steel plate is finally cooled to below 450℃. The organization is mainly lath bainite + martensite.

[0011] b. Pile cooling process: after straightening, the steel plates are placed in a slow cooling pit for stacking and slow cooling. The stack cooling temperature is ≥350℃ and the stack cooling time is ≥48 hours.

[0012] c. Tempering heat treatment, the tempering temperature is controlled at 620-680℃, and the tempering time is controlled at 3.6-4min / mm. It should be noted that after online quenching, the steel plate is mainly composed of larger lath bainite + martensite. In order to eliminate the residual stress generated during online quenching of the steel plate, stabilize the organization and size, obtain the ideal organization dominated by bainite, and make the steel plate achieve the best strength and toughness matching, the steel plate needs to be tempered. Through high-temperature tempering, nitrogen / carbides of microalloying elements V, Nb, and Ti are precipitated in the steel, resulting in the dispersion of heterogeneous particles and intermetallic compounds in the steel matrix. The interaction between these precipitated particles at the grain boundaries and moving dislocations leads to the improvement of mechanical properties such as strength and flow stress of the steel, so that the steel plate meets the requirements of Q550D standard.

[0013] The steel plate obtained according to the above scheme is mainly composed of bainite, containing a small amount of martensite and ferrite, with a yield strength ≥575MPa, a tensile strength ≥710MPa, an elongation after fracture ≥21%, and an impact energy KV2 ≥210J at -20℃. The performance fully meets the requirements of Q550D steel, and the alloy and production costs are much lower than those of similar steel grades. DETAILED DESCRIPTION

[0014] The present solution is further described below in conjunction with specific embodiments.

[0015] (1) Composition design: A Q550D steel plate with a thickness of 50 to 80 mm and a method for producing the same, comprising the following chemical compositions by mass percentage (unit, wt%): C: 0.10 to 0.17, Si: 0.10 to 0.25, Mn: 1.50 to 1.67, P≤0.010, S≤0.005, Als: 0.020 to 0.050, Nb: 0.020 to 0.045, Cr: 0.4 to 0.9, V: 0.050 to 0.080, Ti: 0.010 to 0.020, B: 0.0018 to 0.0022, and the rest are Fe and residual elements. As the thickness of the steel plate changes from 50 mm to 80 mm, the alloy composition also changes from low to high.

[0016] (2) KR molten iron pretreatment: After KR stirring desulfurization, the molten iron S is guaranteed to be ≤0.008% and the desulfurization temperature drop is ≤20℃.

[0017] (3) Converter smelting: S≤0.008% and P≤0.060% of the molten iron, the molten iron temperature≥1300℃, dry high-quality scraps and nickel-containing special scrap steel are selected, and the converter loading is controlled according to the remaining 5-7 tons of steel casting. During the steel tapping process, argon blowing is not allowed, and no deoxidizer or alloy is allowed to be added to the molten steel. At the end of steel tapping, a slag cone is used to block the slag. If the slag blocking fails, the furnace must be lifted in advance to ensure that the thickness of the converter slag is controlled below 20mm to avoid slag rephosphorization.

[0018] (4) Argon blowing treatment: After the molten steel arrives at the argon station and the argon gas is turned on, the aluminum wire is added immediately. The aluminum wire must be fed into the ladle vertically, and it is strictly forbidden to feed the ladle in a spiral manner. After the aluminum wire is added, strong argon blowing is carried out for 3 minutes (the standard for strong argon blowing is to control the total diameter of the naked eye of the blown steel liquid to be controlled within 500-700mm) before leaving the station, and ensure that the leaving station temperature is above 1570℃.

[0019] (5) LF refining: Argon is blown throughout the refining process, and the basicity of the refined slag is controlled at 4.0-6.0. After heating for 3 minutes, 50 kg of calcium carbide is added first, and then 20-40 kg of aluminum particles are added. Thereafter, 2-4 shovels of aluminum particles are added to the ladle with a shovel every 2 minutes to ensure that the slag turns white. In the second heating, 10-30 kg of calcium carbide is added each time according to the arc submergence effect. At the same time, 1-3 shovels of aluminum particles are added to the ladle with a shovel every 2 minutes to ensure that the slag remains white throughout the second heating process. In the third heating, deoxidizer is added according to the color of the slag to maintain white slag. During the refining process, the number of slag sticking is required to be greater than 5 times. Silicon calcium wire is added before leaving the station. Argon must be turned off before adding silicon calcium wire. Vacuum degassing is used, and the leaving station temperature is 1610±10℃.

[0020] (6) VD refining: vacuum degree ≤ 67Pa, pressure holding time ≥ 25min, soft blowing for 3-5min after breaking the air, the molten steel must not be exposed during the soft blowing process, and the H is controlled within 1.8PPm after the vacuum is completed. The covering agent is guaranteed to cover the steel liquid surface. The argon gas must be turned off before adding the covering agent. The leaving station temperature is 1560±15℃.

[0021] (7) Casting: The pouring temperature is controlled at 1560-1565℃, the middle ladle superheat is 15±10℃, the pulling speed is 0.75m / min, the specific water content is 0.80L / kg, the electric stirring is 900A, 5Hz, 30s-3-30s, and the continuous casting requires full protection of the casting. The protective tube must be put in within 1min after the ladle is started. During the pouring of the middle ladle, the steel liquid level must not turn red. During the steel pouring process, the amount of argon blowing from the stopper rod is reasonably controlled to ensure that the liquid level of the crystallizer fluctuates slightly. The billets off the line are stacked and slowly cooled for 48 hours.

[0022] (8) Billet heating: preheating section temperature 900 ~ 1000 ° C, heating section temperature 1260 ~ 1280 ° C, holding section temperature 1240 ~ 1260 ° C, total heating time 10 ~ 13 min / cm.

[0023] (9) Rolling: In the rough rolling stage, "high temperature, low speed and large reduction" rolling is adopted, the starting rolling temperature is ≥1220℃, and the pass reduction is ≥85mm. After rolling, the intermediate billet is cooled to 840-860℃ by IC rapid cooling for the second stage of finishing rolling. High-pressure water cooling is turned on throughout the finishing rolling process. After the final rolling, the temperature of the steel plate is controlled at 820-840℃. After the rolling, the steel plate is relaxed on the roller for 60-80S. After the relaxation, the temperature of the steel plate is controlled at 800-820℃. The steel plate enters NCC rapid cooling at a speed of 0.5m / s, and the cooling rate is controlled at 8-12℃ / S. Finally, the temperature of the steel plate is cooled to below 450℃.

[0024] (10) Stack cooling: After straightening, the steel plates are stacked in a slow cooling pit for slow cooling. The stack cooling temperature is ≥350°C and the stack cooling time is ≥48 hours.

[0025] (11) Tempering heat treatment: The tempering temperature is controlled at 620-680℃, and the tempering time is controlled at 3.6-4min / mm.

[0026] Through the above implementation steps, Q550D steel plates with thicknesses of 55 mm and 80 mm are produced, as follows:

[0027] The chemical composition is shown in Table 1 below.

[0028]

[0029] Tempering process see Table 2 below

[0030] Thickness / mm Tempering temperature / ℃ Time / min Cooling method 55 660-670 200 air cooling 80 640-650 300 air cooling

[0031] The tensile properties are shown in Table 3 below.

[0032] Plate thickness / mm Sampling site Sampling direction <![CDATA[Lower yield strength R cL MPa]]> <![CDATA[Tensile strength R c MPa]]> Elongation after break A% 55 T / 4 Horizontal 610,625,629(621) 745,755,762(754) 22,21,21(21.3) 80 T / 4 Horizontal 590,575,588(584) 725,710,713(716) 24,23,22(23)

[0033] See Table 4 for series low temperature shock

[0034] Plate thickness / mm Sampling site Sampling direction Impact energy KV2 / J Temperature / ℃ 55 T / 4 Vertical 255,265,300(273) -20 80 T / 4 Vertical 245,232,210(229) -20

[0035] Bending properties are shown in Table 5 below

[0036] Plate thickness / mm Sampling site sampling Bend 180° 55 T / 4 Horizontal intact 80 T / 4 Horizontal intact

[0037] In summary, the performance of 55mm / 80mm thick Q550D produced in this trial production is all qualified.

[0038] Surface quality and flaw detection: The surface quality of the steel plate developed is 100% genuine. The flaw detection is carried out according to JB / T 4730, and the first-class rate is 100%, achieving the expected effect.

Claims

1. A method for producing low-cost Q550D steel plate using V instead of Mo, characterized in that: The steel plate has a thickness of 50 to 80 mm and includes the following chemical compositions by mass content (unit, wt%): C: 0.10 to 0.17, Si: 0.10 to 0.25, Mn: 1.50 to 1.67, P≤0.010, S≤0.005, Als: 0.020 to 0.050, Nb: 0.020 to 0.045, Cr: 0.4 to 0.9, V: 0.050 to 0.080, Ti: 0.010 to 0.020, B: 0.0018 to 0.0022, and the rest are Fe and residual elements; The structure of the steel plate is mainly bainite, containing a small amount of martensite and ferrite, with a carbon equivalent Ceq≤0.65, a low welding crack sensitivity coefficient Pcm≤0.30, a yield strength≥575MPa, a tensile strength≥710MPa, an elongation after fracture≥21%, and an impact energy KV2≥210J at -20°C; The production method of the low-cost Q550D steel plate using V instead of Mo includes rolling, stack cooling, and tempering heat treatment, which is specifically as follows: a. Rolling process: in the rough rolling stage, "high temperature, low speed and large reduction" rolling is adopted, the starting rolling temperature is ≥1220℃, and the pass reduction is ≥85mm. After rolling, IC rapid cooling is used to cool the intermediate billet to 840-860℃ for the second stage of finishing rolling. High-pressure water cooling is turned on throughout the finishing rolling process. After the final rolling, the temperature of the steel plate is controlled at 820-840℃. After the rolling, the steel plate is relaxed on the roller for 60-80S. After the relaxation, the temperature of the steel plate is controlled at 800-820℃. The steel plate enters NCC rapid cooling at a speed of 0.5m / s, and the cooling rate is controlled at 8-12℃ / S. Finally, the temperature of the steel plate is cooled to below 450℃; b. Pile cooling process: after straightening, the steel plates are placed in a slow cooling pit for stacking and slow cooling. The stack cooling temperature is ≥350℃ and the stack cooling time is ≥48 hours. c. Tempering heat treatment, the tempering temperature is controlled at 620-680℃, and the tempering time is controlled at 3.6-4min / mm.