Catalyst for selective oxidation of hydrocarbons and its preparation method and application

By using molybdenum disulfide as a lubricant and additive in vanadium phosphorus oxide catalyst, the catalyst deactivation problem caused by excessive graphite introduction is solved, the performance of the catalyst and the selectivity of the manganese are improved, and the efficient n-butane oxidation is achieved. Make the effect.

CN116020505BActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111243331.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-11-05
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

During the process of n-butan oxidation of existing vanadium phosphorus oxide catalysts, excessive use of graphite molding lubricants leads to rapid deactivation and selectivity of the catalyst, and the carbon content of traditional molybdenum additives is present. Influence.

Method used

Molybdenum disulfide (MoS2) is used as a solid lubricant and additive to replace graphite. By introducing Mo additives in the vanadium phosphorus oxide catalyst molding process, an efficient catalyst is formed, reducing the introduction of carbon elements and improving the performance of the catalyst.

Benefits of technology

It is achieved to improve the compressive strength and selectivity of the catalyst, extend the service life of the catalyst and improve the conversion rate while ensuring the catalytic strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020505B_ABST
    Figure CN116020505B_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for selective oxidation of hydrocarbons and its preparation method and application. The catalyst comprises an active phase and an auxiliary phase, wherein the general formula of the active phase is V1P x Mo y C z O u ; The auxiliary agent phase includes molybdenum disulfide. The preparation method includes the steps of: S1, reacting a reaction system containing a vanadium source, a phosphorus source and a solvent to obtain a post-reaction system; S2, performing solid-liquid separation on the post-reaction system to obtain a precursor powder; S3, mixing the precursor powder with molybdenum disulfide to obtain a mixed powder; S4, performing molding on the mixed powder to obtain a catalyst precursor; S5, performing activation on the catalyst precursor to obtain the catalyst. When preparing the catalyst of the present invention, molybdenum disulfide is used instead of graphite as a tableting lubricant to avoid the introduction of too much carbon. The added molybdenum disulfide can not only serve as a tableting lubricant, but also effectively introduce a molybdenum auxiliary agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of chemical synthesis, and in particular to a catalyst for selective oxidation of hydrocarbons and a preparation method and application thereof. Background Art

[0002] Gas phase selective oxidation of hydrocarbons is an important catalytic reaction that can be used to catalyze the preparation of various oxidation products such as organic anhydride compounds. One of the typical products is maleic anhydride (maleic anhydride).

[0003] Maleic anhydride, also known as maleic anhydride (MA), is a commonly used important organic chemical raw material and the third most consumed anhydride variety in the world. Maleic anhydride is currently mainly used in the production of chemicals such as unsaturated polyester resins, alkyd resins, 1,4-butanediol (BDO), γ-butyrolactone (GBL) and tetrahydrofuran (THF). In addition, it is also widely used in various fine chemicals. Especially with the official implementation of the current plastic ban, the demand for degradable plastics is increasing day by day. As one of the important raw materials for degradable plastics, the demand for maleic anhydride will also increase sharply in the future.

[0004] The production of maleic anhydride is mainly divided into two categories. The earliest production method uses benzene as the production raw material, but due to the harmfulness of the raw material itself and the environment, as well as the influence of economic factors, the proportion of the benzene production process in maleic anhydride production has been decreasing. At present, the mainstream production method of maleic anhydride uses n-butane as the production raw material, including fixed bed, fluidized bed, moving bed, etc. These processes have their own characteristics, and most of them have practical industrial applications, but they have one thing in common, that is, these processes for the oxidation of n-butane to produce maleic anhydride all use the same type of catalyst, namely vanadium phosphorus oxide (VPO) catalyst.

[0005] After years of research, it is believed that VPO catalyst is still the most effective catalyst system for catalyzing gas-phase hydrocarbons, especially n-butane to produce maleic anhydride. Industrial VPO catalysts usually use an organic phase method to prepare a precursor, and the resulting precursor is activated by calcination and formed by adding a molding lubricant (generally graphite) to obtain the final catalyst. Previous studies have found that the carbon content in the catalyst has an important impact on the performance of the VPO catalyst (CN1152746C). It can be seen that the addition of molding lubricant graphite will have a significant impact on the performance of the catalyst. The addition of too much graphite may even cause the catalyst to activate and heat up during the reaction process, causing the catalyst to deactivate quickly and the selectivity to decrease. Molybdenum, as a co-catalyst element for oxidation reactions, can adjust the redox ability of the catalyst, reduce the formation of inactive phases, and play a very critical role in the performance of the catalyst. The traditional method of adding molybdenum additives to vanadium phosphorus oxide catalysts is to introduce molybdenum additives by adding molybdenum precursors such as ammonium molybdate or phosphomolybdic acid during the preparation of precursor powder by the organic phase method (CN112705233A and CN112495410A). It is worth pointing out that molybdenum disulfide (MoS2), as a representative molybdenum-containing compound, is a graphite-like material. In adjacent molybdenum disulfide crystals, Mo atomic layers are sandwiched between two layers of tightly packed S atoms to form a layered structure in the form of S-Mo-S, in which Mo-S is strongly covalently bonded, while the S layers are mainly Van der Waals forces. This structure makes it an efficient solid lubricant that can be used for forming and pressing electrode materials and catalysts.

[0006] The inventors found that if MoS2, a solid lubricant, can be used in the molding process of vanadium phosphorus oxide catalyst, it can replace graphite as a tablet molding lubricant to avoid the introduction of excessive carbon. On the other hand, it can also effectively introduce Mo additives in this way, which is expected to improve the performance of the catalyst for the oxidation of n-butane to maleic anhydride. Summary of the invention

[0007] In order to overcome the problems existing in the prior art, the inventors of the present invention have conducted extensive and in-depth research and provided a catalyst for the selective oxidation of hydrocarbons and a preparation method and application thereof. For example, one of the purposes of the present invention is to provide a catalyst for the selective oxidation of hydrocarbons, which can achieve the introduction of a molybdenum additive while ensuring the catalytic strength, so as to obtain a high-yield catalyst for the selective oxidation of hydrocarbons.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a catalyst for selective oxidation of hydrocarbons, comprising an active phase and an additive phase. The general formula of the active phase is shown in formula (I):

[0009] V1P x Mo y C z Ou Formula (I)

[0010] In formula (I), the value range of x is 0.5 to 2, the value range of y is 0.01 to 0.1, the value range of z is 0 to 0.02, and u is the number of oxygen atoms that satisfies the valence of the active phase.

[0011] According to the present invention, preferably, the value range of x is 0.95 to 1.6.

[0012] According to the present invention, the catalyst may be referred to as a vanadium phosphorus oxide catalyst.

[0013] According to the present invention, through X-ray diffraction analysis, the XRD diffraction spectrum of the catalyst has diffraction peaks belonging to the molybdenum compound at 2θ angles of 14.4±0.3, 32.7±0.3, 35.9±0.3 and 39.5±0.3.

[0014] According to the present invention, the molybdenum compound is mainly molybdenum disulfide.

[0015] In some embodiments of the present invention, based on the total weight of the catalyst, the mass percentage of the active phase in the catalyst is 90% to 99.5%; the mass percentage of the auxiliary phase is 0.5% to 5%.

[0016] In some embodiments of the present invention, the mass percentage of carbon element in the catalyst is no more than 5%.

[0017] According to the present invention, carbon element is neither an active phase nor an auxiliary phase.

[0018] According to the present invention, during the preparation process, the C-containing raw materials, solvents or gases in the reaction atmosphere will introduce carbon elements into the catalyst.

[0019] In some embodiments of the present invention, the compressive strength of the catalyst is 15N to 30N.

[0020] According to the present invention, the ZQJ-II intelligent particle strength testing machine of Dalian Intelligent Testing Machine Factory is used, and the test standard method is based on "Application of ZQJ Intelligent Particle Strength Testing Machine" in "China Petroleum and Chemical Standards and Quality" (1991, No. 3, pp. 31-33, 28, a total of 4 pages), to obtain the compressive strength of the catalyst.

[0021] The second aspect of the present invention provides a method for preparing the catalyst according to the first aspect of the present invention, comprising the steps of:

[0022] S1, reacting a reaction system containing a vanadium source, a phosphorus source and a solvent to obtain a reaction system;

[0023] S2, performing solid-liquid separation treatment on the reaction system to obtain a precursor powder;

[0024] S3, mixing the precursor powder with molybdenum disulfide to obtain a mixed powder;

[0025] S4, performing molding treatment on the mixed powder to obtain a catalyst precursor;

[0026] S5, performing activation treatment on the catalyst precursor to obtain the catalyst.

[0027] In some embodiments of the present invention, in step S1, the vanadium source is selected from at least one of vanadium pentoxide, ammonium metavanadate and organic vanadium acid, preferably vanadium pentoxide.

[0028] In some embodiments of the present invention, the phosphorus source is phosphoric acid, preferably 85 to 110 wt % of phosphoric acid, more preferably 95 to 105 wt % of phosphoric acid.

[0029] In some embodiments of the present invention, the solvent is selected from at least one of a monohydric alcohol and a polyhydric alcohol, preferably a mixture of isobutyl alcohol and benzyl alcohol, preferably, the molar ratio of isobutyl alcohol to benzyl alcohol in the mixture is 2:1 to 6:1. In the reaction system, the molar ratio of vanadium element to phosphorus element is (0.6 to 1.1): 1. In the reaction system, the ratio of the total mass of the solvent to the total mass of the vanadium source is (5 to 10): 1.

[0030] In some embodiments of the present invention, in step S1, the reaction conditions include: a temperature of 100°C to 120°C.

[0031] The present invention has no special requirements on the reaction pressure. Preferably, the reaction in step S1 is carried out under normal pressure.

[0032] According to the present invention, in step S1, a reaction system containing a vanadium source, a phosphorus source and a solvent may be mixed and then heated to reflux for 2 to 20 hours.

[0033] According to the present invention, the solvent may also function as a reducing agent. It should be noted that if the added solvent cannot function as a reducing agent, an additional reducing agent may be added. The type of reducing agent is not particularly limited, and those skilled in the art may use substances commonly used in the art.

[0034] In some embodiments of the present invention, in step S2, the solid-liquid separation treatment can be carried out by filtration, evaporation, etc. For example, the post-reaction system obtained in step S1 is filtered and washed with a solvent (a solution having at least one same component as the solvent in step S1), and the obtained filter cake can be dried at 120°C for 16 hours.

[0035] In some embodiments of the present invention, in step S3, the amount of molybdenum disulfide added is 0.5% to 5% by mass of the precursor powder, preferably 1% to 3%.

[0036] According to the present invention, in step S3, the purity of the molybdenum disulfide is greater than 95%.

[0037] In some embodiments of the present invention, in step S4, the molding process includes sequentially performing a first tableting process on the precursor powder using a powder tablet press at a pressure of 10 to 40 MPa, and then performing crushing, screening and a second tableting process. Preferably, the screening includes screening out catalyst particles with a particle size of 20 to 160 mesh and performing a subsequent second tableting process thereon, so as to obtain a hollow cylindrical catalyst to be activated with a height of 4 to 6 mm.

[0038] According to the present invention, in step S4, the screened catalyst particles with a mesh size of 20 to 160 may be placed on a rotary tablet press for a second tableting process.

[0039] The present invention has no particular limitation on the crushing method and conditions, and those skilled in the art can select a suitable process according to the target product.

[0040] In some embodiments of the present invention, in step S5, the activation treatment is performed in an atmosphere formed by one or more of an oxygen-containing gas, an inert gas and water vapor; preferably, the inert gas is at least one of nitrogen, helium and argon.

[0041] According to the present invention, in step S5, the catalyst precursor may be activated three times in an atmosphere formed by one or more of an oxygen-containing gas, an inert gas and water vapor.

[0042] According to the present invention, in step S5, the activation treatment is performed three times, the first time is performed in an air atmosphere at 200°C to 350°C for 2 to 5 hours; the second time is performed in an atmosphere with a volume content of 15% to 25% air, 15% to 25% nitrogen, 5% to 15% carbon dioxide and 45% to 55% water vapor at 300°C to 450°C for 2 to 5 hours; the third time is performed in an atmosphere with a volume content of 35% to 45% nitrogen, 5% to 15% carbon dioxide and 45% to 55% water vapor at 400°C to 450°C for 2 to 5 hours.

[0043] In some embodiments of the present invention, the method for preparing the catalyst comprises the steps of:

[0044] 1) mixing a vanadium compound, phosphoric acid and an organic solvent as a reducing agent and a solvent, and heating under reflux for 2 to 20 hours to obtain a reaction solution;

[0045] 2) filtering the reaction solution and washing it with the same organic solvent as in step 1), and then heat-treating the filter cake at 100° C. to 120° C. to obtain a precursor powder;

[0046] 3) The precursor powder is mixed evenly with molybdenum disulfide, and subjected to pre-granulation and secondary tableting to obtain a hollow cylindrical catalyst to be activated with a height of 4 to 6 mm;

[0047] 4) The hollow cylindrical catalyst to be activated is subjected to activation treatment in an atmosphere consisting of oxygen-containing gas, inert gas and water vapor to obtain the catalyst.

[0048] The third aspect of the present invention provides an application of the catalyst described in the first aspect of the present invention and / or the catalyst prepared by the preparation method described in the second aspect in the selective oxidation of hydrocarbons, especially in the catalytic oxidation of n-butane to produce maleic anhydride.

[0049] In some embodiments of the present invention, the catalyst is used to produce maleic anhydride by gas phase catalytic oxidation using n-butane as a raw material, including: placing the catalyst in a fixed bed reactor, the reaction atmosphere includes n-butane with a molar concentration of 1% to 1.7%, and producing maleic anhydride by thermal catalysis. The process conditions for the reaction include: a space velocity of 1000-3000 hr -1 , the reaction temperature is 300°C to 500°C, and the reaction pressure is normal pressure.

[0050] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0051] 1) The catalyst provided by the present invention has a promoter phase of molybdenum disulfide, and the catalyst contains less carbon element;

[0052] 2) The preparation method of the catalyst provided by the present invention avoids the introduction of excessive graphite carbon by using molybdenum disulfide instead of graphite as a tableting lubricant;

[0053] 3) In the preparation method of the catalyst provided by the present invention, the added molybdenum disulfide can not only be used as a tableting lubricant, but also effectively introduce a molybdenum additive;

[0054] 4) When the catalyst provided by the present invention is used in the catalytic oxidation of n-butane to produce maleic anhydride, the butane conversion rate is high, the maleic anhydride selectivity is high, and the yield is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0056] Figure 1 The XRD spectrum of the catalyst prepared in Example 1 of the present invention is shown;

[0057] Figure 2 The XRD spectrum of the catalyst prepared in Comparative Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0058] The present invention is described in detail below by way of examples, but the protection scope of the present invention is not limited to the following description.

[0059] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. The raw materials, reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained through commercial channels or prepared according to the preparation methods disclosed in the prior art.

[0060] In the embodiment, the calculation method of butane conversion is:

[0061] Butane conversion rate (%) = molar amount of n-butane consumed in the reaction / molar amount of raw material n-butane fed × 100%.

[0062] In the embodiment, the calculation method of maleic anhydride selectivity is:

[0063] Maleic anhydride selectivity (%) = molar amount of maleic anhydride produced / molar amount of n-butane consumed in the reaction × 100%.

[0064] Example 1

[0065] 1. Preparation of catalyst

[0066] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of isobutyl alcohol and 1000ml of benzyl alcohol, stirring is started and about 300g of 100wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutyl alcohol, and the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 5g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A1.

[0067] The catalyst product A1 was subjected to strength analysis and the compressive strength was measured to be 23N.

[0068] The catalyst product A1 was subjected to X-ray diffraction analysis, and the results were as follows: Figure 1 As shown. Figure 1 It can be seen that there are main diffraction characteristic peaks at 2θ=12.5, 14.4, 18.5, 22.8, 28.4, 29.3, 29.9, 32.7, 35.9, 39.5, 43.2 and 49.8, among which the peaks of 2θ=14.4, 32.7, 35.9 and 39.5 belong to the diffraction peaks of molybdenum compounds.

[0069] 2. Catalytic reaction

[0070] The obtained catalyst product A1 was fed with 1.5 vol% butane for 2000 hr -1 The butane conversion was 85.8% and the maleic anhydride selectivity was 63.1% when evaluated in a fixed bed reactor at a low space velocity.

[0071] Example 2

[0072] 1. Preparation of catalyst

[0073] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of isobutyl alcohol and 800ml of benzyl alcohol, stirring is started and about 350g of 110wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutyl alcohol, the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 5g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A2.

[0074] The catalyst product A2 was subjected to strength analysis and the compressive strength was measured to be 22N.

[0075] 2. Catalytic reaction

[0076] The obtained catalyst product A2 was fed with 1.5 vol% butane for 2000 hr -1 The butane conversion was 84.9% and the maleic anhydride selectivity was 62.8% when evaluated in a fixed bed reactor at a low space velocity.

[0077] Example 3

[0078] 1. Preparation of catalyst

[0079] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of isobutyl alcohol and 800ml of benzyl alcohol, stirring is started and about 320g of 110wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutyl alcohol, the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 10g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A3.

[0080] The catalyst product A3 was subjected to strength analysis and the compressive strength was measured to be 24N.

[0081] 2. Catalytic reaction

[0082] The obtained catalyst product A3 was fed with 1.5 vol% butane for 2000 hr -1 The butane conversion was 85.9% and the maleic anhydride selectivity was 62.1% when evaluated in a fixed bed reactor at a low space velocity.

[0083] Example 4

[0084] 1. Preparation of catalyst

[0085] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of isobutyl alcohol and 800ml of benzyl alcohol, stirring is started and about 280g of 110wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutyl alcohol, the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 5g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A4.

[0086] The catalyst product A4 was subjected to strength analysis and the compressive strength was measured to be 22N.

[0087] 2. Catalytic reaction

[0088] The obtained catalyst product A4 was fed with 1.5 vol% butane for 2000 hr -1 The butane conversion was 83.9% and the maleic anhydride selectivity was 62.5% when evaluated in a fixed bed reactor at a low space velocity.

[0089] Example 5

[0090] 1. Preparation of catalyst

[0091] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of isobutyl alcohol and 800ml of benzyl alcohol, stirring is started and about 300g of 110wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutyl alcohol, and the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 2g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A5.

[0092] The catalyst product A5 was subjected to strength analysis and the compressive strength was measured to be 18N.

[0093] 2. Catalytic reaction

[0094] The obtained catalyst product A5 was fed with 1.5 vol% butane for 2000 hr -1 The butane conversion was 83.4% and the maleic anhydride selectivity was 62.1% when evaluated in a fixed bed reactor at a low space velocity.

[0095] Example 6

[0096] 1. Preparation of catalyst

[0097] 320g of ammonium metavanadate is added to a mixed solution of 2500ml of isobutanol and 1000ml of benzyl alcohol, stirring is started and about 300g of 100wt.% phosphoric acid is slowly added, the mixed solution is heated to 110°C, refluxed for 16h, the mixed solution is filtered after heating is stopped and washed with isobutanol, and the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 5g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A6.

[0098] The catalyst product A6 was subjected to strength analysis and the compressive strength was measured to be 22N.

[0099] 2. Catalytic reaction

[0100] The obtained catalyst product A6 was evaluated in a fixed bed reactor with 1.5 vol% butane feed and a space velocity of 2000 hr-1. The butane conversion was measured to be 84.8% and the maleic anhydride selectivity was 62.0%.

[0101] Example 7

[0102] 1. Preparation of catalyst

[0103] 250g of vanadium pentoxide is added to a mixed solution of 2500ml of ethylene glycol and 1000ml of benzyl alcohol, stirring is started and about 300g of 100wt.% phosphoric acid is slowly added, heated to reflux and refluxed for 16h, the mixed solution is filtered and washed with isobutyl alcohol after heating is stopped, and the filter cake is dried at 120°C for 16h to obtain a precursor powder. The precursor powder is sieved to obtain a precursor powder less than 200 mesh, 5g of molybdenum disulfide compound is taken and mixed with 250g of precursor powder less than 200 mesh to form a mixed powder. The mixture is tableted at a pressure of 20MPa, then crushed and sieved, and the 20-160 mesh portion after sieving is taken, and the above pre-granulated particles are transferred to a rotary tablet press, the catalyst structure height is 5mm, and the catalyst precursor is obtained by rotary tableting. The catalyst precursor was calcined at 250°C in an air atmosphere for 3 hours, then heated to 425°C in an atmosphere of 20% air, 20% nitrogen, 10% carbon dioxide and 50% water vapor by volume and calcined for 3 hours, and finally calcined at 450°C in an atmosphere of 40% nitrogen, 10% carbon dioxide and 50% water vapor by volume for 3 hours to obtain catalyst product A7.

[0104] The catalyst product A7 was subjected to strength analysis and the strength was measured to be 21N.

[0105] 2. Catalytic reaction

[0106] The obtained catalyst product A6 was evaluated in a fixed bed reactor with 1.5 vol% butane feed and a space velocity of 2000 hr-1. The butane conversion was measured to be 83.9% and the maleic anhydride selectivity was 61.1%.

[0107] Comparative Example 1

[0108] 1. Preparation of catalyst

[0109] The process is basically the same as Example 1, except that 6 g of graphite powder is used instead of 5 g of molybdenum disulfide compound in Example 1 to obtain catalyst product B1.

[0110] The catalyst product B1 was subjected to strength analysis and the compressive strength was measured to be 25N.

[0111] The catalyst product B1 was subjected to X-ray diffraction analysis, and the results were as follows: Figure 2 As shown. Figure 2 It can be seen that there are main diffraction characteristic peaks at 2θ=12.5, 18.5, 22.8, 26.5, 28.4, 29.3, 29.9, 43.2 and 49.8, among which the peak of 2θ=26.5 belongs to the diffraction peak of graphite carbon. It can be found that in the catalyst product using graphite as a tableting lubricant, the diffraction peak intensity of carbon is relatively large.

[0112] 2. Catalytic reaction

[0113] The obtained catalyst product B1 was evaluated in a fixed bed reactor with 1.5 vol% butane feed and a space velocity of 2000 hr-1. The butane conversion was measured to be 84.8% and the maleic anhydride selectivity was 59.9%.

[0114] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A catalyst for selective oxidation of hydrocarbons, comprising an active phase and a promoter phase, wherein: The general formula of the active phase is shown in formula (I): V1P x Mo y C z O u Formula (I) In formula (I), x is in the range of 0.5 to 2, y is in the range of 0.01 to 0.1, z is in the range of 0 to 0.02, and u is the number of oxygen atoms that satisfies the valence of the active phase; The additive phase includes molybdenum disulfide.

2. The catalyst according to claim 1, characterized in that Taking the total weight of the catalyst as a calculation basis, in the catalyst, the mass percentage of the active phase is 90% to 99.5%; the mass percentage of the auxiliary agent phase is 0.5% to 5%.

3. The catalyst according to claim 1 or 2, characterized in that The mass percentage of carbon element in the catalyst is not more than 5%.

4. The catalyst according to any one of claims 1 to 3, characterized in that The compressive strength of the catalyst is 15N-30N.

5. A method for preparing the catalyst according to any one of claims 1 to 4, comprising the steps of: S1, reacting a reaction system containing a vanadium source, a phosphorus source and a solvent to obtain a reaction system; S2, performing solid-liquid separation treatment on the reaction system to obtain a precursor powder; S3, mixing the precursor powder with molybdenum disulfide to obtain a mixed powder; S4, performing molding treatment on the mixed powder to obtain a catalyst precursor; S5, performing activation treatment on the catalyst precursor to obtain the catalyst.

6. The preparation method according to claim 5, characterized in that: In step S1, the vanadium source is selected from at least one of vanadium pentoxide, ammonium metavanadate and organic vanadium acid; and / or The phosphorus source is phosphoric acid; and / or The solvent is selected from at least one of a monohydric alcohol and a polyhydric alcohol; and / or In the reaction system, the molar ratio of vanadium to phosphorus is (0.6-1.1):1; and / or In the reaction system, the ratio of the total mass of the solvent to the total mass of the vanadium source is (5-10):

1.

7. The preparation method according to claim 6, characterized in that: In step S1, the vanadium source is vanadium pentoxide; and / or The phosphorus source is 85-110 wt % phosphoric acid; and / or The solvent is a mixture of isobutyl alcohol and benzyl alcohol.

8. The preparation method according to claim 7, characterized in that: The phosphorus source is 95-105 wt % phosphoric acid; and / or The molar ratio of isobutanol to benzyl alcohol in the mixture is 2:1 to 6:

1.

9. The preparation method according to any one of claims 5 to 8, characterized in that: In step S1, the reaction conditions include: a temperature of 100°C to 120°C.

10. The preparation method according to any one of claims 5 to 8, characterized in that: In step S3, the mass of the added molybdenum disulfide is 0.5% to 5% of the mass of the precursor powder.

11. The preparation method according to claim 10, characterized in that: In step S3, the mass of the added molybdenum disulfide is 1% to 3% of the mass of the precursor powder.

12. The preparation method according to any one of claims 5 to 8, characterized in that: In step S4, the molding process includes sequentially performing a first tableting process, crushing, screening, and a second tableting process on the precursor powder.

13. The preparation method according to claim 12, characterized in that: The screening includes screening out catalyst particles with a particle size of 20 to 160 meshes and performing a subsequent second tabletting process.

14. The preparation method according to any one of claims 5 to 8, characterized in that: In step S5, the activation treatment is carried out in an atmosphere formed by one or more of an oxygen-containing gas, an inert gas and water vapor; and / or The temperature of the activation treatment is 370° C. to 480° C., and the time of the activation treatment is 1 to 20 hours.

15. The preparation method according to claim 14, characterized in that: The inert gas is at least one of nitrogen, helium and argon.

16. Use of the catalyst according to any one of claims 1 to 4 and / or the catalyst prepared by the preparation method according to any one of claims 5 to 15 in the selective oxidation of hydrocarbons.

17. The use according to claim 16, characterized in that The catalyst is used in preparing maleic anhydride by catalytic oxidation of n-butane.