Aluminum phosphate sol and preparation method thereof, catalytic cracking aid, catalytic cracking catalyst and application thereof, and method for catalytic conversion of hydrocarbon oil

By using a specific composition aluminum phosphate sol as a binder, combining cracking active components and clay, the problem of poor selectivity of propylene in the prior art is solved, and the production of propylene and isobutene during catalytic cracking is improved. The rate and concentration achieve the distribution of high value-added products.

CN116020534BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111258122.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-12
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

The existing phosphorus-containing aluminum adhesive additives have poor propylene selectivity during catalytic cracking, making it difficult to effectively improve the yield and concentration of propylene.

Method used

Aluminum phosphate sol with a specific composition is used as a binder to form an aluminum phosphate sol by contacting the phosphoric acid solution with an aluminum source and used to prepare a catalytic cracking additive, combining cracking active components and clay to form a high bonding performance and stable catalytic cracking catalyst.

Benefits of technology

The yield and concentration of propylene and isobutene during catalytic cracking is improved, the selectivity of the catalyst is enhanced, and the catalyst strength and high value-added product distribution are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020534B_ABST
    Figure CN116020534B_ABST
Patent Text Reader

Abstract

The invention relates to the field of aluminum phosphate sol, and discloses aluminum phosphate sol and a preparation method thereof, a catalytic cracking aid, a catalytic cracking catalyst and its application, and a method for catalytic conversion of hydrocarbon oil. The aluminum phosphate compound contained in the aluminum phosphate sol contains polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compound, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compound is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%. It has the characteristics of longer storage time and more stability. It is used for catalytic cracking conversion of hydrocarbon oil, has higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are improved to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalytic cracking aids, and in particular to an aluminum phosphate sol and a preparation method thereof, a catalytic cracking aid containing the aluminum phosphate sol, a catalytic cracking catalyst containing the catalytic cracking aid, applications of the catalytic cracking aid and the catalytic cracking catalyst, and a method for catalytic conversion of hydrocarbon oil using the catalytic cracking aid and the catalytic cracking catalyst. Background Art

[0002] Propylene is one of the most important organic chemical raw materials. Its largest use is the production of polypropylene, accounting for about 52%, followed by the production of acrylonitrile 12%, propylene oxide 7%, isopropyl benzene 7%, isopropyl alcohol 4%, carbonyl alcohol 9% and other 9%. With the development of the national economy, the demand for propylene has increased dramatically. In recent years, the growth rate of propylene demand has been higher than that of ethylene. Fluidized catalytic cracking is one of the important production processes for light olefins and propylene. It can increase the production of propylene by using catalytic cracking units without making major adjustments to the production equipment and processes.

[0003] The use of propylene-increasing additives is currently the most effective way to increase the yield of light olefins in catalytic cracking units. Currently, most catalysts or additives used to increase propylene production in catalytic cracking units use ZSM-5 molecular sieves, and in order to further improve the reaction performance of propylene additives, it is usually necessary to modify the ZSM-5 molecular sieve or directly modify the additives, among which phosphorus modification is the main modification method.

[0004] USP5997728 discloses a method for increasing olefin production by using an additive in the catalytic cracking process of heavy raw materials. The additive is a ZSM-5 zeolite with 12-40 wt% added to an amorphous matrix.

[0005] US3758403 discloses using ZSM-5 as an active component for increasing propylene production, and using ZSM-5 together with ReY molecular sieve as active components to prepare FCC catalysts.

[0006] CN100537030C discloses a catalyst promoter for increasing the propylene concentration of catalytic cracking liquefied gas, which contains, based on the weight of the promoter, 10-655% of MFI structure zeolite, 0-20% of non-MFI structure zeolite, 0-60% of clay, 15-60% of inorganic oxide binder in terms of oxide, 0.5-15% of copper additive in terms of CuO, and 2-25% of phosphorus additive in terms of P2O5. The catalyst promoter is applied in the catalytic cracking process of petroleum hydrocarbons, and can significantly increase the propylene concentration in the liquefied gas while increasing the yield of catalytic cracking liquefied gas and improving the octane number of catalytic cracking gasoline.

[0007] In order to further improve the propylene yield of the catalytic promoter, the prior art often uses a phosphate aluminum gel binder, but the existing promoter containing the phosphate aluminum gel binder still has the problem of poor propylene selectivity. Summary of the invention

[0008] The purpose of the present invention is to overcome the problem that the existing additives of aluminum phosphate adhesives still have poor propylene selectivity, and to provide an aluminum phosphate sol and a preparation method thereof, a catalytic cracking additive, a catalytic cracking catalyst and its application, and a method for catalytic conversion of hydrocarbon oil.

[0009] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an aluminum phosphate sol, wherein the aluminum phosphate compound contained in the aluminum phosphate sol contains polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compound, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compound is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%.

[0010] A second aspect of the present invention provides a method for preparing aluminum phosphate sol, wherein the method comprises:

[0011] (1) bringing a phosphoric acid solution into first contact with a first aluminum source to obtain a first slurry;

[0012] (2) contacting the first slurry with a second aluminum source to obtain an aluminum phosphate sol.

[0013] The third aspect of the present invention provides an aluminum phosphate sol prepared by the method of the present invention.

[0014] The fourth aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-55wt% of cracking active components, 5-30wt% of clay and 15-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol provided by the present invention.

[0015] The fifth aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.

[0016] A sixth aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil.

[0017] A seventh aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting the hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction.

[0018] Through the above technical scheme, the present invention provides an aluminum phosphate sol with a specific composition, which has the characteristics of long storage time and more stability. The catalytic cracking aid further prepared is used for catalytic cracking conversion of hydrocarbon oil, especially for catalytic cracking of heavy oil, which can have a high distribution of high value-added products while ensuring the strength of the catalyst, and can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, it can increase the isobutylene yield and the isobutylene concentration in the catalytic cracking liquefied gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is the TEM image of sample PA-5;

[0020] Figure 2 It is the sample of PA-1, PA-DB-1 and PA-DB-2. 31 P-NMR spectrum. DETAILED DESCRIPTION

[0021] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0022] The first aspect of the present invention provides an aluminum phosphate sol, wherein the aluminum phosphate sol contains aluminum phosphate compounds containing polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compounds, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compounds is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%.

[0023] The composition of the aluminum phosphate sol provided by the present invention may include phosphoric acid and its polymers (polyphosphoric acid, polymers between phosphoric acids) and aluminum phosphate compounds. The aluminum phosphate compound contains polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate. The monohydroxy aluminum phosphate refers to an aluminum phosphate compound containing one hydroxyl group. The polyhydroxy aluminum phosphate refers to an aluminum phosphate compound containing two or more hydroxyl groups.

[0024] In the present invention, the phosphate aluminum gel 31 P-NMR assignment , where m and n represent the number of Al-OP bonds and POP bonds, respectively. 31 In the P-NMR spectrum, polyhydroxyaluminum phosphate refers to the region with a chemical shift of -8 ppm. and a chemical shift at -13 ppm Monohydroxyaluminum phosphate refers to the chemical shift at -12ppm Hydroxy-free aluminum phosphate refers to the chemical shift at -17ppm The content of each of the above aluminum phosphate compounds can be obtained by NUTS peak fitting. and The content of aluminum phosphate compounds (except 0ppm The mass percentage of monohydroxy aluminum phosphate refers to Total aluminum phosphate compounds (except 0ppm The mass percentage of hydroxy-free aluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of phosphoric acid.

[0025] In the present invention, the aluminum phosphate sol preferably does not contain chlorine and nitrate. The aluminum phosphate sol also contains water.

[0026] In some embodiments of the present invention, preferably, based on the total amount of the aluminum phosphate compound, the content of the polyhydroxy aluminum phosphate in the aluminum phosphate compound is 60-91wt% and the content of the monohydroxy aluminum phosphate is 0.5-20wt%. The aluminum phosphate sol having the above-mentioned polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate content can have a strong bonding performance and a larger particle size, and can be further used to obtain a catalytic cracking aid that can provide a technical effect of improving propylene selectivity. Wherein, the content of the hydroxy-free aluminum phosphate is 8-20wt%.

[0027] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, based on the total amount of the aluminum phosphate sol, the content of the aluminum phosphate compound is 50-70wt%, preferably 60-67wt%. In addition, the content of phosphoric acid contained in the aluminum phosphate sol may be 7-30wt%, and the content of polyphosphoric acid may be 18-30wt%.

[0028] In some embodiments of the present invention, preferably, based on the total amount of the aluminum phosphate sol, the Al element content is 5-15wt%, preferably 7-11wt%, and the P element content is 20-30wt%, preferably 25-27wt%.

[0029] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3.6:1, preferably 2-3:1. The above elemental composition can be determined by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).

[0030] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 20-40wt%, preferably 21-26wt%. Solid content refers to the total mass content of Al2O3 and P2O5 in the aluminum phosphate sol, which can be determined by the method of calcination at 800°C for 1h.

[0031] In some embodiments of the present invention, preferably, the viscosity of the aluminum phosphate sol is 1500-7000 mPa·s, preferably 2000-4000 mPa·s. Viscosity refers to dynamic viscosity, which can be measured by a Thermo Scientific HAAKE VT550 rotational viscometer, using a 3# rotor, at 20°C and a shear rate of 2900 r / min.

[0032] The aluminum phosphate sol with the above composition and performance parameters provided by the present invention can have stronger bonding performance and better stability, and the particle size of the colloid particles is large and relatively uniform, with an average particle size of 30-55nm, which can reduce the blockage of the molecular sieve pores and acid sites, give full play to the role of the molecular sieve, and is conducive to being used as a catalytic cracking aid in the catalytic cracking reaction of hydrocarbon oil to obtain products, thereby increasing the concentration of propylene and isobutylene in liquefied petroleum gas.

[0033] A second aspect of the present invention provides a method for preparing aluminum phosphate sol, wherein the method comprises:

[0034] (1) bringing a phosphoric acid solution into first contact with a first aluminum source to obtain a first slurry;

[0035] (2) contacting the first slurry with a second aluminum source to obtain an aluminum phosphate sol.

[0036] In some embodiments of the present invention, step (1) is used to fully react the aluminum source to generate aluminum dihydrogen phosphate compounds with high hydroxyl content and good adhesion. Preferably, in step (1), the concentration of the phosphoric acid solution is 15-85wt%, preferably 15-30wt%.

[0037] In some embodiments of the present invention, preferably, the temperature of the first contact does not exceed 80°C, preferably 55-75°C; the time of the first contact is more than 30 min, preferably 15-120 min, more preferably 30-60 min.

[0038] In some embodiments of the present invention, preferably, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus-aluminum molar ratio of the first slurry is 2-10, preferably 4-7. Preferably, the first aluminum source is added to the phosphoric acid solution and stirred thoroughly.

[0039] In some embodiments of the present invention, preferably, the solid content of the first slurry is 25-35wt%, preferably 27-34wt%.

[0040] In some embodiments of the present invention, preferably, the viscosity of the first slurry is 500-700 mPa·s, preferably 550-650 mPa·s.

[0041] In some embodiments of the present invention, preferably, in step (2), the temperature of the second contact does not exceed 80°C, preferably 55-75°C; the time of the second contact is more than 30 minutes, preferably 30-120 minutes, more preferably 60-90 minutes.

[0042] In some embodiments of the present invention, preferably, the second aluminum source is added to the first slurry and mixed with sufficient stirring.

[0043] In some embodiments of the present invention, preferably, the aluminum introduced by the first aluminum source accounts for 1 / 2-5 / 6 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source, preferably 3 / 5-4 / 5. The amount of the second aluminum source added satisfies the composition of the aluminum phosphate sol finally obtained, the molar ratio of P:Al is 1.6-3.6:1 as mentioned above, preferably 2-3:1, and has the physicochemical properties such as solid content and viscosity as mentioned above, and can provide the catalytic cracking aid in the catalytic conversion of hydrocarbon oil, in combination with other components to achieve improved selectivity of propylene, and the isobutylene yield in the obtained liquefied gas product is high.

[0044] In some embodiments of the present invention, preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of elemental aluminum, aluminum oxide, hydrated aluminum oxide that can be colloided by acid and / or aluminum salts, and can be the above pure substances or a slurry or solution after the pure substances are mixed and slurried with water.

[0045] In the present invention, the elemental aluminum can be selected from at least one of aluminum sheets and aluminum particles; the aluminum oxide can be selected from at least one of γ-alumina, ρ-alumina, χ-alumina, η-alumina, κ-alumina, δ-alumina, and θ-alumina; the acid-colloidable hydrated aluminum oxide can be selected from at least one of gibbsite, diaspore, boehmite, and pseudo-boehmite; the aluminum salt can be selected from at least one of aluminum chloride, aluminum nitrate, and aluminum sulfate.

[0046] Preferably, the aluminum source is pseudo-boehmite.

[0047] In the present invention, the water used as a solvent in the phosphoric acid solution, and the water used as a solvent in the first aluminum source and the second aluminum source, which may be a slurry or a solution, may be acidic water, i.e., decationized water, preferably with a pH value of 3-5, and a sodium oxide content of preferably <5 ppm by mass.

[0048] The third aspect of the present invention provides an aluminum phosphate sol prepared by the method of the present invention.

[0049] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 20-40 wt %, preferably 21-26 wt %.

[0050] In some embodiments of the present invention, preferably, the viscosity of the aluminum phosphate sol is 1500-7000 mPa·s, preferably 2000-4000 mPa·s.

[0051] In some embodiments of the present invention, preferably, the composition of the prepared aluminum phosphate sol is as described above and will not be repeated herein.

[0052] The fourth aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-55wt% of cracking active components, 5-30wt% of clay and 15-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol provided by the present invention.

[0053] In the present invention, preferably, in the composition of the catalytic cracking aid, the total content of the cracking active component, clay and binder can be 100wt%.

[0054] In some embodiments of the present invention, preferably, the cracking active component is selected from at least one of shape selective zeolite, MCM zeolite and L zeolite, preferably shape selective zeolite.

[0055] Preferably, the framework type of the shape-selective zeolite is an MFI structure, preferably a ZSM-5 zeolite, more preferably a modified ZSM-5 zeolite or a HZSM-5 zeolite.

[0056] Preferably, the modifying element contained in the modified ZSM-5 zeolite is selected from at least one of P, Fe, Co, Mn, Ni, Ga, Zn, Cu, Ti, K, Mg and RE, preferably selected from at least one of P, Fe, Mn, Ga, Cu and RE.

[0057] Preferably, in the modified ZSM-5 zeolite, the content of the modifying element is ≤10 wt%, preferably ≤5 wt%.

[0058] Preferably, the molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50, preferably 22-32.

[0059] In the present invention, the above-mentioned modifying elements contained in the modified ZSM-5 zeolite can be added in a step-by-step manner. For example, at least one of ZRP-1, ZRP-5, ZSP-3, ZSP-4 and MPZ molecular sieves is selected, and then other required modifying elements are added. The above-mentioned molecules can be commercially available, such as the ZRP-1 molecular sieve provided by the Qilu Branch of Sinopec Catalyst Co., Ltd., which can contain P modification. Other required modifying elements, such as Fe element, are added to the ZRP-1 molecular sieve as needed.

[0060] In some embodiments of the present invention, preferably, the binder further comprises other binders, and the other binders are selected from at least one of alumina sol, pseudo-boehmite and silica sol.

[0061] In some embodiments of the present invention, preferably, based on the total dry weight of the binder, the content of the other binders in the binder is 0-40 wt %, and the content of the aluminum phosphate sol is 60-100 wt %.

[0062] In some embodiments of the present invention, preferably, based on the total dry weight of the catalytic cracking aid, the content of the aluminum phosphate sol is 24-50wt%, preferably 28-45wt%.

[0063] In some embodiments of the present invention, preferably, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay, preferably selected from at least one of kaolin, metakaolin and diatomaceous earth.

[0064] The present invention also provides a method for preparing the above catalytic cracking aid, comprising: mixing cracking active components, a binder, clay and water to form a slurry, drying and roasting, and then washing and drying after washing to obtain the catalytic cracking aid.

[0065] Wherein, the cracking active component can be as described above, preferably a modified ZSM-5 zeolite. It can be modified by multiple steps so that the modified ZSM-5 zeolite contains the modified elements required by the present invention. Commercially available, such as ZRP-1 molecular sieve, already contains P element, and then the molecular sieve is contacted with an aqueous solution of a compound containing the modified element required by the present invention for modification, and the obtained slurry is then mixed with a binder, clay and water. Wherein, in the final modified ZSM-5 zeolite, the content of the modified element (the total amount of multiple elements) is ≤10wt%, preferably ≤5wt%.

[0066] In the present invention, the drying temperature is 80-200°C, preferably 80-120°C. The time can be selected according to actual needs, and there is no specific limitation on this. The amount of each component used to form the slurry satisfies the composition of the obtained catalytic cracking aid and meets the requirements of the aforementioned catalytic cracking aid, which will not be repeated here. The roasting conditions can refer to the technical conditions in the art, for example, the roasting temperature can be 500-600°C, and the roasting time can be 4-12h.

[0067] In the present invention, in the preparation method, the washing can be carried out by water washing and / or ammonium washing, and the technical conditions in the art can be referred to, for example, two water washings and one ammonium washing, the water / agent weight ratio (the weight ratio of water to the spherical catalyst particles obtained by roasting) during water washing is (5-10):1, and the temperature is 60-90°C; the ammonium / agent ratio (the weight ratio of ammonium ions in the aqueous solution containing ammonium compounds to the spherical catalyst particles obtained by roasting) during ammonium washing is 1:(50-100). The drying after washing can be, for example, air flow drying or drying, for example, drying at 100-120°C.

[0068] The fifth aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.

[0069] It may also be a catalytic cracking aid prepared by the aforementioned preparation method of the catalytic cracking aid.

[0070] In some embodiments of the present invention, preferably, based on the total weight of the catalytic cracking catalyst, the content of the main catalyst in the catalytic cracking catalyst is 80-95wt%, preferably 85-92wt%; the content of the auxiliary agent is 5-20wt%, preferably 8-15wt%.

[0071] The main catalyst may be a conventional catalytic cracking catalyst in the art, which can be purchased commercially, such as a catalyst with the brand name HBC produced by Sinopec Catalyst Co., Ltd.

[0072] The sixth aspect of the present invention provides a catalytic cracking aid or a catalytic cracking catalyst provided by the present invention for use in a catalytic reaction of hydrocarbon oil. The hydrocarbon oil can be selected from petroleum and its various fractions, and is particularly suitable for petroleum fractions with a boiling point greater than 330°C, such as one or more of atmospheric residue, vacuum residue, atmospheric wax oil, straight run wax oil, and coker wax oil.

[0073] The seventh aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction. The reaction may be a catalytic cracking reaction, and the reaction conditions may include: a reaction temperature of 350-800°C, preferably 450-650°C; and a catalyst-oil ratio of 2-25, preferably 2-6.

[0074] In the present invention, when the catalytic cracking adjuvant or catalytic cracking catalyst containing the above-mentioned aluminum phosphate sol is used to carry out catalytic cracking reaction, the distribution of products that can be obtained by treating the above-mentioned hydrocarbon oil can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, the butene yield, especially the isobutylene yield, can be increased, and the isobutylene concentration in the catalytic cracking liquefied gas can be increased. In particular, when used for catalytic cracking of heavy oil, the product has a higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are both improved to a certain extent.

[0075] In the present invention, the room temperature is 10-25°C.

[0076] The present invention will be described in detail below by way of examples. The specifications of the raw materials used in the examples are as follows:

[0077] Pseudo-boehmite: Shanxi Jinlu of China Aluminum Corporation, Al2O3 content 66.36wt%;

[0078] Concentrated phosphoric acid: chemically pure, concentration 85wt%, produced by Beijing Chemical Plant;

[0079] Kaolin: solid content 78wt%, produced by Suzhou Kaolin Company;

[0080] ZRP-1 molecular sieve: produced by Sinopec Catalyst Co., Ltd., Na2O is 0.06wt%, SiO2 / Al2O3 molar ratio is 25, crystallinity is 87%, P modification, content is 1.3wt%;

[0081] Acidic water, decationized water, pH 4.5;

[0082] Industrial catalyst: produced by Sinopec Catalyst Co., Ltd., brand name HBC.

[0083] The components of the catalyst obtained in the examples are determined by calculation based on the feed amounts of the various raw materials.

[0084] Analytical methods:

[0085] (1) The composition of each material was analyzed by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).

[0086] (2)27 Al-NMR and 31 P-NMR used Varian INOVA II 500MHz superconducting nuclear magnetic resonance spectrometer to test the liquid sample of the prepared aluminum phosphate sol. The experimental conditions were: resonance frequency 130MHz, spectral width 200ppm (mass), sampling times 3000 times, delay time 2s, sampling time 5.6ms, rotation speed 20Hz, and the resonance spectrum was peak-fitted and the peak area was calculated by integration method.

[0087] (3) The size of the colloidal particles was measured using a JEM-2000FX-II transmission electron microscope from Japan Electronics Co., Ltd. The sample was prepared by suspension in distilled water and then quickly fixed by alcohol drying. The accelerating voltage was 120 kV. The average particle size of the colloidal particles was obtained by randomly measuring more than 10 colloidal particle projections in the sample TEM image and taking the average value of the maximum circumscribed circle diameter.

[0088] (4) Viscosity is dynamic viscosity, which was measured using a Thermo Scientific HAAKE VT550 rotational viscometer with a 3# rotor at 20°C and a shear rate of 2900 r / min.

[0089] (5) Stability time: the time during which the prepared aluminum phosphate sol remains in a good sol state at room temperature without stratification.

[0090] In the following examples, the room temperature is 10-25°C.

[0091] Examples 1-5 illustrate the preparation of the aluminum phosphate sol provided by the present invention.

[0092] Example 1

[0093] (1) 53.4 g of phosphoric acid was added to 240 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 27 wt %), and stirred for 10 min. Then 17.8 g of pseudo-boehmite was added, stirred, and the temperature was raised to 55° C. and stirred at 55° C. for 30 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.1, the solid content was 33.6 wt %, and the viscosity was 580 mPa·s);

[0094] (2) 7.6 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 55° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-1.

[0095] Example 2

[0096] (1) 58 g of phosphoric acid was added to 294 g of acidic water and mixed at 20° C. (to obtain a phosphoric acid solution with a concentration of 20 wt %), and stirred for 7 min. Then, 12.9 g of pseudo-boehmite was added, stirred, and the temperature was raised to 75° C. and stirred for 60 min at 75° C. to obtain a first slurry (with a phosphorus-aluminum molar ratio of 6.2, a solid content of 27.4 wt %, and a viscosity of 600 mPa·s);

[0097] (2) 6.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 75° C. for 60 min to obtain an aluminum phosphate sol, which was recorded as PA-2.

[0098] Example 3

[0099] (1) 55.8 g of phosphoric acid was added to 295 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 19 wt %), and stirred for 5 min. Then 17.8 g of pseudo-boehmite was added, stirred, and the temperature was raised to 65° C. and stirred at 65° C. for 45 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.3, the solid content was 27.5 wt %, and the viscosity was 553 mPa·s);

[0100] (2) 4.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 65° C. for 75 min to obtain an aluminum phosphate sol, which was recorded as PA-3.

[0101] Example 4

[0102] (1) 49.7 g of phosphoric acid was added to 241 g of acidic water and mixed at 18° C. (the concentration of the phosphoric acid solution was 21 wt %), and stirred for 5 min. Then, 15.5 g of pseudo-boehmite was added, stirred, and the temperature was raised to 60° C. and stirred at 60° C. for 30 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.4, the solid content was 27.7 wt %, and the viscosity was 572 mPa·s);

[0103] (2) 15.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 60° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-4.

[0104] Example 5

[0105] (1) 60 g of phosphoric acid was added to 294 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 21 wt %), and stirred for 7 min. Then 14.1 g of pseudo-boehmite was added, stirred, and the temperature was raised to 65° C. and stirred at 65° C. for 40 min to obtain a first slurry (with a phosphorus-aluminum molar ratio of 5.8, a solid content of 28.3 wt %, and a viscosity of 650 mPa·s);

[0106] (2) 3 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 65° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-5.

[0107] Comparative Example 1

[0108] 21.1 g of pseudo-boehmite (on a dry basis, the same below), 25.8 g of kaolin and 168 g of acidic water were mixed and stirred at 20°C for 30 minutes, 75.6 g of phosphoric acid was added, and then the temperature was raised to 70°C. After the temperature stabilized at 70°C, stirring was continued for 90 minutes to obtain a product recorded as PA-DB-1.

[0109] Comparative Example 2

[0110] 22.3 g of pseudo-boehmite was mixed with 295 g of acidic water at 20°C, stirred and slurried for 30 minutes, 38.6 g of phosphoric acid was poured into the pseudo-boehmite slurry and stirred at 20°C for 30 minutes, and then 20 g of phosphoric acid was added and stirred at 60°C for 90 minutes to obtain a product recorded as PA-DB-2.

[0111] The physicochemical properties of the aluminum phosphate sols obtained in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1, and the TEM image of PA-5 in Example 5 is shown in Figure 1 , PA-1 of Example 1, PA-DB-1 of Comparative Example 1, and PA-DB-2 of Comparative Example 2 31 P-NMR peak fitting diagram is shown in Figure 2 .

[0112] Table 1

[0113]

[0114] Note: 1 :Content of aluminum phosphate compound in aluminum phosphate sol

[0115] The phosphate aluminum gel in the present invention 31 P-NMR assignment , where m and n represent the number of Al-OP bonds and POP bonds, respectively. 31 In the P-NMR spectrum, polyhydroxyaluminum phosphate refers to the region with a chemical shift of -8 ppm. and a chemical shift at -13 ppm Monohydroxyaluminum phosphate refers to the chemical shift at -12ppm Hydroxy-free aluminum phosphate refers to the chemical shift at -17ppm The content of each substance is obtained by NUTS peak fitting. The content of polyhydroxy aluminum phosphate refers to and The content of aluminum phosphate compounds (except 0ppm The mass percentage of monohydroxy aluminum phosphate refers to Total aluminum phosphate compounds (except 0ppm The mass percentage of hydroxy-free aluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of phosphoric acid.

[0116] From Table 1 and Figure 2 It can be seen that compared with the comparative example, the aluminum phosphate sol provided by the present invention and The polyhydroxy aluminum phosphate compound has a high content, the proportion of which is greater than 60wt%, a high hydroxyl content, and good bonding performance. The aluminum phosphate sol provided by the present invention has a long stability time and a high viscosity, and can maintain its good bonding performance for a long time. Moreover, if Figure 1 As shown, the aluminum phosphate sol provided by the present invention has a larger and more uniform particle size, which can reduce the blockage of the molecular sieve pores and acid sites.

[0117] Examples 6-12 illustrate the preparation of the catalytic cracking aid provided by the present invention.

[0118] Example 6

[0119] 150g of ZRP-1 molecular sieve (on a dry basis, the same below) and 9g of Fe(NO3)3 were mixed and slurried in 265g of water for 30 minutes to obtain a molecular sieve slurry; wherein, the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 3.3wt%, becoming a modified zeolite.

[0120] 21g of kaolin (on a dry basis, the same below), 437g of acidic water, and 12g of pseudo-boehmite (on a dry basis, the same below) were mixed and slurried for 30 minutes, 2.4g of hydrochloric acid was added and stirred for 30 minutes, and then 78g of aluminum phosphate sol PA-1 (on a dry basis, the same below), 36g of aluminum sol (on a dry basis, the same below) and the above molecular sieve slurry were added and stirred for 30 minutes, and spray-dried to prepare a microsphere catalyst.

[0121] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 solution at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, and then washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z1. The proportions are shown in Table 2.

[0122] Example 7

[0123] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed with 212g of water and slurried for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0124] 39g kaolin, 479g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-1, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.

[0125] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z2. The proportions are shown in Table 2.

[0126] Example 8

[0127] 90g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed and slurried in 159g of water for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 4.6wt%, becoming a modified zeolite.

[0128] 39g kaolin, 527g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 78g aluminum phosphate sol PA-1, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray dried to obtain a microsphere catalyst.

[0129] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z3. The proportions are shown in Table 2.

[0130] Example 9

[0131] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed with 212g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0132] 39g kaolin, 479g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-2, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.

[0133] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to a (NH4)2SO4: microsphere catalyst mass ratio of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z4, and its proportion is shown in Table 2.

[0134] Example 10

[0135] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed with 212g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0136] 39g kaolin, 479g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-3, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.

[0137] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to a (NH4)2SO4: microsphere catalyst mass ratio of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z5, and its proportion is shown in Table 2.

[0138] Embodiment 11

[0139] 90g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed and slurried in 159g of water for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 4.6wt%, becoming a modified zeolite.

[0140] 78 g of kaolin was mixed with 538 g of acidic water and slurried for 30 min, 129 g of aluminum phosphate sol PA-1 and the above molecular sieve slurry were added and stirred for 30 min, and then spray-dried to prepare a microsphere catalyst.

[0141] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z6. The proportions are shown in Table 2.

[0142] Example 12

[0143] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed and slurried in 212g of water for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0144] 39g kaolin, 471g acidic water and 15g pseudo-boehmite were mixed and slurried for 30min, 3g hydrochloric acid was added and stirred for 30min, then 96g aluminum phosphate sol PA-1, 27g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray dried to obtain a microsphere catalyst.

[0145] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named Z7. The proportions are shown in Table 2.

[0146] Comparative Example 3

[0147] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed with 212g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0148] 39g kaolin, 479g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-DB-1, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.

[0149] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to a (NH4)2SO4: microsphere catalyst mass ratio of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named DB1, and its proportion is shown in Table 2.

[0150] Comparative Example 4

[0151] 120g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed with 212g of water and beaten for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added made the modifying elements added to the ZRP-1 molecular sieve to be P and Fe, and the content was 3.8wt%, becoming a modified zeolite.

[0152] 39g kaolin, 479g acidic water and 24g pseudo-boehmite were mixed and slurried for 30min, 4.8g hydrochloric acid was added and stirred for 30min, then 72g aluminum phosphate sol PA-DB-2, 36g aluminum sol and the above molecular sieve slurry were added and stirred for 30min, and spray-dried to prepare a microsphere catalyst.

[0153] The microsphere catalyst was calcined at 500°C for 4h, then washed once with (NH4)2SO4 at 80°C according to a (NH4)2SO4: microsphere catalyst mass ratio of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named DB2, and its proportion is shown in Table 2.

[0154] Comparative Example 5

[0155] 90g of ZRP-1 molecular sieve and 9g of Fe(NO3)3 were mixed and slurried in 159g of water for 30 minutes to obtain molecular sieve slurry, wherein the amount of Fe(NO3)3 added was such that the modifying elements added to the ZRP-1 molecular sieve were P and Fe, and the content was 4.6wt%, becoming a modified zeolite.

[0156] 78 g of kaolin was mixed with 538 g of acidic water and slurried for 30 min, 129 g of aluminum phosphate sol PA-DB-2 and the above molecular sieve slurry were added and stirred for 30 min, and then spray-dried to prepare a microsphere catalyst.

[0157] The microsphere catalyst was calcined at 500°C for 4 hours, then washed once with (NH4)2SO4 at 80°C according to the mass ratio of (NH4)2SO4: microsphere catalyst of 1:100, washed twice with water at 80°C until the Na2O content was less than 0.2wt%, filtered and dried at 120°C to obtain a catalytic cracking aid containing aluminum phosphate sol, named DB3. The proportions are shown in Table 2.

[0158] Table 2

[0159]

[0160] Note: *The modified zeolite is ZRP-1 molecular sieve (already containing P modification, P content is 1.3wt%) and then modified with Fe.

[0161] ** is the amount of Fe added in the modified zeolite.

[0162] Catalyst reaction evaluation method:

[0163] Z1-Z7, DB1-DB3 and industrial catalyst were mixed in a mass ratio of 1:9 to obtain catalytic cracking catalysts C1-C7 and D1-D3. The composition of the industrial catalyst is shown in Table 3.

[0164] Table 3

[0165]

[0166] The composition of the catalytic feedstock oil is shown in Table 4.

[0167] Table 4

[0168]

[0169]

[0170] The catalytic cracking catalysts C1-C7 and D1-D3 prepared above were aged at 800°C and 100% steam for 17 h, respectively, and then filled into a small fixed fluidized bed ACE device (purchased from KTI, USA), with a filling amount of 9 g each. Then, at a reaction temperature of 510°C and a weight hourly space velocity of 12 h -1 The catalyst-oil ratio (weight) was 3, and the catalytic raw oil was injected into the ACE device for catalytic cracking reaction. The reaction results are shown in Table 5.

[0171] The composition of the reaction products is analyzed, including dry gas, liquefied gas, gasoline, diesel, heavy oil and coke, and the catalytic cracking reaction conversion rate of the feedstock oil is calculated according to the following formula:

[0172]

[0173] Liquefied gas contains propylene and C4 olefins. The composition of C4 olefins includes: 1-butene, isobutylene, cis-2-butene and trans-2-butene.

[0174]

[0175]

[0176] Table 5

[0177]

[0178] As can be seen from Table 5, the additive prepared by using the aluminum phosphate sol provided by the present invention can have a higher distribution of high value-added products while ensuring the strength of the catalyst (larger pore volume and lower wear index than the comparative example), and can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, it can increase the isobutylene yield and the isobutylene concentration in the catalytic cracking liquefied gas.

[0179] The additive provided by the present invention has a higher propylene yield and isobutylene yield under the same formula (other components are the same) compared with the additive prepared by aluminum phosphate sol provided by the prior art (as shown in Comparative Examples 3, 4, and 5), and has a better economic value. When the molecular sieve content is low (such as Example 8 compared with Examples 6 and 7), a better propylene yield and isobutylene yield (higher than the comparative example) can also be guaranteed.

[0180] When the binder in the auxiliary agent provided by the present invention is only the aluminum phosphate sol of the present invention, the product obtained by the catalytic cracking reaction of the crude oil has a higher propylene yield (Example 11), a significantly higher isobutylene yield, and the isobutylene concentration in the liquefied gas is significantly higher.

[0181] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An aluminum phosphate sol, characterized in that The aluminum phosphate compound contained in the aluminum phosphate sol contains polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compound, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compound is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%; in the aluminum phosphate sol, based on the total amount of the aluminum phosphate sol, the content of the aluminum phosphate compound is 50-70wt%; in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3.6:

1.

2. The aluminum phosphate sol according to claim 1, wherein Based on the total amount of the aluminum phosphate compound, the content of the polyhydroxy aluminum phosphate in the aluminum phosphate compound is 60-91wt% and the content of the monohydroxy aluminum phosphate is 0.5-20wt%; And / or, in the aluminum phosphate sol, the content of the aluminum phosphate compound is 60-67wt% based on the total amount of the aluminum phosphate sol.

3. The aluminum phosphate sol according to claim 1 or 2, wherein In the aluminum phosphate sol, the molar ratio of P:Al is 2-3:1; and / or, based on the total amount of the aluminum phosphate sol, the Al content is 5-15wt%, and the P content is 20-30wt%; And / or, the solid content of the aluminum phosphate sol is 20-40wt%; And / or, the viscosity of the aluminum phosphate sol is 1500-7000 mPa·s.

4. The aluminum phosphate sol according to claim 3, wherein Based on the total amount of the aluminum phosphate sol, the Al element content is 7-11wt%, and the P element content is 25-27wt%; and / or, the solid content of the aluminum phosphate sol is 21-26wt%; And / or, the viscosity of the aluminum phosphate sol is 2000-4000 mPa·s.

5. A method for preparing the aluminum phosphate sol according to any one of claims 1 to 4, characterized in that: The method includes: (1) contacting a phosphoric acid solution with a first aluminum source to obtain a first slurry; (2) The first slurry is brought into second contact with a second aluminum source to obtain an aluminum phosphate sol.

6. The method according to claim 5, wherein: In step (1), the concentration of the phosphoric acid solution is 15-85wt%; And / or, the temperature of the first contact does not exceed 80°C; the time of the first contact is more than 30 minutes; and / or, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus to aluminum molar ratio of the first slurry is 2-1; and / or, the solid content of the first slurry is 25-35wt%; And / or, the viscosity of the first slurry is 500-700 mPa·s.

7. The method according to claim 6, wherein: In step (1), the concentration of the phosphoric acid solution is 15-30wt%; And / or, the temperature of the first contact is 55-75°C; the time of the first contact is 15-120 minutes; and / or, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus to aluminum molar ratio of the first slurry is 4-7; and / or, the solid content of the first slurry is 27-34wt%; And / or, the viscosity of the first slurry is 550-650 mPa·s.

8. The method according to claim 7, wherein: In step (1), the first contacting time is 30-60 minutes.

9. The method according to any one of claims 5 to 8, wherein: In step (2), the temperature of the second contact is no more than 80°C; the time of the second contact is more than 30 minutes; and / or, the aluminum introduced by the first aluminum source accounts for 1 / 2-5 / 6 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source; And / or, the first aluminum source and the second aluminum source are each independently selected from at least one of elemental aluminum, aluminum oxide, hydrated aluminum oxide, and aluminum salt.

10. The method according to claim 9, wherein: In step (2), the temperature of the second contact is 55-75°C; the time of the second contact is 30-120 minutes; And / or, the aluminum introduced by the first aluminum source accounts for 3 / 5-4 / 5 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source.

11. The method according to claim 10, wherein: In step (2), the second contact time is 60-90 minutes.

12. A catalytic cracking aid, characterized in that: Based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-55wt% of cracking active components, 5-30wt% of clay and 15-50wt% of a binder; wherein the binder comprises the aluminum phosphate sol according to any one of claims 1-4.

13. The catalytic cracking aid according to claim 12, wherein: The cracking active component is at least one selected from the group consisting of shape-selective zeolite, MCM zeolite, and L zeolite; And / or, the binder further comprises other binders, and the other binders are selected from at least one of alumina sol, pseudo-boehmite and silica sol; And / or, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.

14. The catalytic cracking aid according to claim 13, wherein The cracking active component is shape-selective zeolite; and / or, based on the total dry weight of the binder, the content of the other binders in the binder is 0-40wt%, and the content of the aluminum phosphate sol is 60-100wt%; And / or, the clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.

15. The catalytic cracking aid according to claim 13 or 14, wherein: The framework type of the shape-selective zeolite is an MFI structure.

16. The catalytic cracking aid according to claim 15, wherein The shape selective zeolite is ZSM-5 zeolite.

17. The catalytic cracking aid according to claim 16, wherein: The shape selective zeolite is modified ZSM-5 zeolite or HZSM-5 zeolite.

18. The catalytic cracking aid according to claim 17, wherein The modified ZSM-5 zeolite contains at least one modifying element selected from the group consisting of P, Fe, Co, Mn, Ni, Ga, Zn, Cu, Ti, K, Mg and RE.

19. The catalytic cracking aid according to claim 18, wherein The modified ZSM-5 zeolite contains at least one modified element selected from the group consisting of P, Fe, Mn, Ga, Cu and RE.

20. The catalytic cracking aid according to any one of claims 17 to 19, wherein: In the modified ZSM-5 zeolite, the content of the modifying element is ≤10wt%.

21. The catalytic cracking aid according to any one of claims 13-14, 16-19, wherein: The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.

22. The catalytic cracking aid according to claim 21, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.

23. The catalytic cracking aid according to claim 15, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.

24. The catalytic cracking aid according to claim 23, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.

25. The catalytic cracking aid according to claim 20, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 20-50.

26. The catalytic cracking aid according to claim 25, wherein The molar ratio of SiO2 / Al2O3 of the shape selective zeolite is 22-32.

27. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, wherein the auxiliary agent is the catalytic cracking auxiliary agent described in any one of claims 12-26.

28. The catalytic cracking catalyst according to claim 27, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 80-95wt%; and the content of the auxiliary agent is 5-20wt%.

29. The catalytic cracking catalyst according to claim 28, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 85-92wt%; and the content of the auxiliary agent is 8-15wt%.

30. Use of the catalytic cracking aid according to any one of claims 12 to 26, or the catalytic cracking catalyst according to any one of claims 27 to 29 in a catalytic reaction of hydrocarbon oil.

31. A method for catalytic conversion of hydrocarbon oil, comprising: The hydrocarbon oil is contacted with the catalytic cracking aid described in any one of claims 12 to 26, or with the catalytic cracking catalyst described in any one of claims 27 to 29 for reaction.