Catalytic cracking aid, catalytic cracking catalyst and application thereof, and method for catalytic conversion of hydrocarbon oil
By using a specific aluminum phosphate sol as a binder in the catalytic cracking additive, the selectivity of C4 olefins and the yield of isobutene are improved, and the problem of poor isobutene concentration and propylene selectivity in the prior art is solved, and the problem of poor isobutene concentration and propylene selectivity is achieved. Efficient catalytic cracking effect.
Patent Information
- Application Number
- CN202111258062.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The existing catalytic cracking additives have poor effect in isobutene concentration and propylene selectivity, and the coke yield is high, making it difficult to meet the demand for improving the yield and concentration of C4 olefins.
A catalytic cracking additive is provided, containing 25-35% by weight of cracking active components, 20-55% by weight of clay and 20-50% by weight of aluminum phosphate sol as binder, and the aluminum phosphate sol contains polyhydroxy aluminum phosphate and monohydrate. Aluminum hydroxyphosphate can improve its stability and bonding properties through specific preparation methods.
The selectivity and yield of C4 olefins are significantly improved, the yield and concentration of isobutene is increased, the yield and concentration of coke is decreased, and the concentration of C4 olefins in the liquefied gas is increased.
Smart Images

Figure CN116020538B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalytic cracking aids, and in particular to a catalytic cracking aid, a catalytic cracking catalyst containing the catalytic cracking aid, applications of the catalytic cracking aid and the catalytic cracking catalyst, and a method for catalytic conversion of hydrocarbon oil using the catalytic cracking aid and the catalytic cracking catalyst. Background Art
[0002] The global oil supply is becoming increasingly tight, and the profit margins of oil refining companies are becoming narrower and narrower. C4 olefins are important organic chemical raw materials, and the global demand for C4 olefins is increasing year by year. Due to the restrictions on the content of olefins and aromatics in National VI gasoline, alkylation gasoline is the most suitable blending product of National VI gasoline. The raw materials of alkylation gasoline are mainly C4 olefins, and FCC increasing the production of C4 olefins is one of the processes. For most catalytic cracking units, adding additives is an effective technical approach to increase the production of C4 olefins. However, the existing technology has no obvious effect on increasing the concentration of isobutylene. From the perspective of isobutylene generation and reaction chemistry in the FCC process, Beta molecular sieve is an effective active component, and phosphorus compounds are introduced into the matrix to improve the selectivity of the catalyst for C4 olefins.
[0003] US6355591 discloses a catalytic cracking aid, which contains 4-20% aluminum phosphate, 1-40% ZSM-5, Beta and a mixture thereof, and 40-90% clay, and can increase LPG production. The preparation method of aluminum phosphate is: concentrated phosphoric acid is added to deionized water for dilution, and aluminum powder is added to dissolve, wherein the molar ratio of Al to PO4 is 1:3, and the pH is less than 2.0. The prepared aluminum phosphate is evenly mixed with kaolin, and then mixed into the molecular sieve slurry, and finally sprayed into shape. The aid does not contain other binders or other inorganic oxides except aluminum phosphate. In addition, the preparation method and performance of the aid containing Beta zeolite are not given in the examples.
[0004] CN103771437A discloses a phosphorus-containing modified Beta molecular sieve, wherein the phosphorus content is 3-10% by weight based on P2O5. 27 In Al MAS NMR, the ratio of the peak area of the resonance signal with a chemical shift of 40±3ppm to the peak area of the resonance signal with a chemical shift of 54ppm±3ppm is greater than or equal to 1. The phosphorus in the molecular sieve is fully coordinated with the framework aluminum, the framework aluminum is fully protected, and the molecular sieve has excellent hydrothermal stability and better product selectivity.
[0005] CN103785456A discloses a cracking aid for increasing the concentration of light olefins, comprising a modified beta molecular sieve, a phosphorus-aluminum inorganic binder containing a first clay, other inorganic binders and a Group VIII metal additive, with or without a second clay; the phosphorus-aluminum inorganic binder containing the first clay comprises an aluminum component, a phosphorus component and the first clay; the phosphorus-and-transition metal modified beta molecular sieve has a phosphorus content of 1-10% by weight in terms of P2O5 and a metal content of 0.5-10% by weight in terms of metal oxide. The cracking catalyst composition is applied to the catalytic cracking of petroleum hydrocarbons, can increase the yield of catalytic cracking liquefied gas, increase the concentration of light olefins in the liquefied gas, especially the concentration of isobutylene, and at the same time increase the ratio of ethylene to dry gas, increase the octane number of gasoline, and do not affect the heavy oil conversion ability of the main catalyst when the additive is mixed in a large proportion.
[0006] CN107971023B discloses a catalytic cracking aid containing phosphorus-containing and metal-loaded Beta molecular sieve and a preparation method thereof. The aid contains 10-75% by weight of phosphorus-containing and metal-loaded Beta molecular sieve on a dry basis, 3-30% by weight of a phosphorus-aluminum inorganic binder containing a first clay on a dry basis, 3-30% by weight of other inorganic binders on an oxide basis, 0-60% by weight of a second clay on a dry basis, and 0-15% by weight of a Group VIII metal additive on an oxide basis, by weight and based on the dry basis weight of the aid. The aid is applied to catalytic cracking to increase the yield of isobutylene and propylene and improve the octane number of gasoline.
[0007] CN104998681B discloses a catalytic cracking aid for increasing the concentration of light olefins and a preparation method thereof. The aid comprises a boron-modified phosphorus- and metal-containing Beta molecular sieve, an inorganic oxide binder, a Group VIII metal additive, a phosphorus additive, and optional clay. The catalytic cracking aid is applied to the catalytic cracking of petroleum hydrocarbons, can increase the concentration of isobutylene in the catalytic cracking liquefied gas, and reduce the production of coke.
[0008] However, the product distribution obtained when catalytic cracking is carried out using the above-mentioned additives is still not ideal. Summary of the invention
[0009] The purpose of the present invention is to overcome the problems that the existing additives containing phosphorus aluminum gel binder still have low isobutylene concentration in the liquefied gas obtained by catalytic cracking, poor propylene selectivity and high coke yield, and to provide a catalytic cracking additive, a catalytic cracking catalyst and its application and a method for catalytic conversion of hydrocarbon oil.
[0010] In order to achieve the above object, the first aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-35wt% of a cracking active component, 20-55wt% of clay and 20-50wt% of a binder; wherein the binder comprises aluminum phosphate sol;
[0011] Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into Beta zeolite;
[0012] The aluminum phosphate sol contains aluminum phosphate compounds including polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compounds, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compounds is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%.
[0013] The second aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.
[0014] The third aspect of the present invention provides a use of the catalytic cracking aid or catalytic cracking catalyst provided by the present invention in a catalytic reaction of hydrocarbon oil.
[0015] A fourth aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting the hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction.
[0016] Through the above technical solution, the catalytic cracking aid provided by the present invention contains an aluminum phosphate sol with a specific composition. The aluminum phosphate sol has the characteristics of longer storage time and greater stability, and can bring about higher C4 olefin selectivity, C4 olefin yield and concentration effects for the use of the catalytic cracking aid.
[0017] The hydrocarbon oil catalytic conversion method provided by the present invention can be used for hydrocarbon oil catalytic cracking conversion, especially for heavy oil catalytic cracking reaction. The catalytic cracking catalyst containing the above-mentioned catalytic cracking adjuvant of the present invention has a higher selectivity for C4 olefins while ensuring the isobutylene yield and concentration, so that the C4 olefin yield and concentration are improved to a certain extent, the liquefied gas can have a higher C4 olefin concentration, and surprisingly, has a higher isobutylene yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is the TEM image of sample PA-5;
[0019] Figure 2It is the sample of PA-1, PA-DB-1 and PA-DB-2. 31 P-NMR spectrum. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] The first aspect of the present invention provides a catalytic cracking aid, wherein, based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-35wt% of a cracking active component, 20-55wt% of clay and 20-50wt% of a binder; wherein the binder comprises aluminum phosphate sol;
[0022] Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta type zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into the Beta type zeolite;
[0023] The aluminum phosphate sol contains aluminum phosphate compounds including polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compounds, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compounds is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%.
[0024] The composition of the aluminum phosphate sol provided by the present invention may include phosphoric acid and its polymers (polyphosphoric acid, polymers between phosphoric acids) and aluminum phosphate compounds. The aluminum phosphate compound contains polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate. The monohydroxy aluminum phosphate refers to an aluminum phosphate compound containing one hydroxyl group. The polyhydroxy aluminum phosphate refers to an aluminum phosphate compound containing two or more hydroxyl groups.
[0025] In the present invention, the phosphate aluminum gel 31 P-NMR assignment , where m and n represent the number of Al-OP bonds and POP bonds, respectively. 31 In the P-NMR spectrum, polyhydroxyaluminum phosphate refers to the region with a chemical shift of -8 ppm. and a chemical shift at -13 ppm Monohydroxyaluminum phosphate refers to the chemical shift at -12ppm Hydroxy-free aluminum phosphate refers to the chemical shift at -17ppm The content of each of the above aluminum phosphate compounds can be obtained by NUTS peak fitting. and The content of aluminum phosphate compounds (except 0ppm The mass percentage of monohydroxyaluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of hydroxy-free aluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of phosphoric acid.
[0026] In the present invention, the aluminum phosphate sol preferably does not contain chlorine and nitrate. The aluminum phosphate sol also contains water.
[0027] In some embodiments of the present invention, preferably, based on the total amount of the aluminum phosphate compound, the content of the polyhydroxy aluminum phosphate in the aluminum phosphate compound is 60-91wt% and the content of the monohydroxy aluminum phosphate is 0.5-20wt%. The aluminum phosphate sol having the above-mentioned polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate content can have a strong bonding performance and a larger particle size, and can be further used to obtain a catalytic cracking aid that can have a technical effect of improving the selectivity of carbon four olefins. Wherein, the content of the hydroxy-free aluminum phosphate is 8-20wt%.
[0028] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, based on the total amount of the aluminum phosphate sol, the content of the aluminum phosphate compound is 50-70wt%, preferably 60-67wt%. In addition, the content of phosphoric acid contained in the aluminum phosphate sol may be 7-30wt%, and the content of polyphosphoric acid may be 18-30wt%.
[0029] In some embodiments of the present invention, preferably, based on the total amount of the aluminum phosphate sol, the Al element content is 5-15wt%, preferably 7-11wt%, and the P element content is 20-30wt%, preferably 25-27wt%.
[0030] In some embodiments of the present invention, preferably, in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3.6:1, preferably 2-3:1. The above elemental composition can be determined by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).
[0031] In some embodiments of the present invention, preferably, the solid content of the aluminum phosphate sol is 20-40wt%, preferably 21-26wt%. Solid content refers to the total mass content of Al2O3 and P2O5 in the aluminum phosphate sol, which can be determined by the method of calcination at 800°C for 1h.
[0032] In some embodiments of the present invention, preferably, the viscosity of the aluminum phosphate sol is 1500-7000 mPa·s, preferably 2000-4000 mPa·s. Viscosity refers to dynamic viscosity, which can be measured by a Thermo Scientific HAAKE VT550 rotational viscometer, using a 3# rotor, at 20°C and a shear rate of 2900 r / min.
[0033] The catalytic cracking aid provided by the present invention contains aluminum phosphate sol having the above physicochemical properties, which can help improve the selectivity of C4 olefins in the catalytic conversion of hydrocarbon oil, and the isobutylene yield in the obtained liquefied gas product is relatively high.
[0034] In some embodiments of the present invention, preferably, the method for preparing the aluminum phosphate sol comprises:
[0035] (1) bringing a phosphoric acid solution into first contact with a first aluminum source to obtain a first slurry;
[0036] (2) contacting the first slurry with a second aluminum source to obtain the aluminum phosphate sol.
[0037] In some embodiments of the present invention, step (1) is used to fully react the aluminum source to generate aluminum dihydrogen phosphate compounds with high hydroxyl content and good adhesion. Preferably, in step (1), the concentration of the phosphoric acid solution is 15-85wt%, preferably 15-30wt%.
[0038] In some embodiments of the present invention, preferably, the temperature of the first contact does not exceed 80°C, preferably 55-75°C; the time of the first contact is more than 30 min, preferably 15-120 min, more preferably 30-60 min.
[0039] In some embodiments of the present invention, preferably, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus-aluminum molar ratio of the first slurry is 2-10, preferably 4-7. Preferably, the first aluminum source is added to the phosphoric acid solution and stirred thoroughly.
[0040] In some embodiments of the present invention, preferably, the solid content of the first slurry is 25-35wt %, preferably 27-34wt %.
[0041] In some embodiments of the present invention, preferably, the viscosity of the first slurry is 500-700 mPa·s, preferably 550-650 mPa·s. The conditions for implementing the above step (1) can provide aluminum phosphate sol with the final performance.
[0042] In some embodiments of the present invention, preferably, in step (2), the temperature of the second contact does not exceed 80°C, preferably 55-75°C; the time of the second contact is more than 30 minutes, preferably 30-120 minutes, more preferably 60-90 minutes.
[0043] In some embodiments of the present invention, preferably, the second aluminum source is added to the first slurry and mixed with sufficient stirring.
[0044] In some embodiments of the present invention, preferably, the aluminum introduced by the first aluminum source accounts for 1 / 2-5 / 6 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source, preferably 3 / 5-4 / 5. The amount of the second aluminum source added satisfies the composition of the aluminum phosphate sol finally obtained, the molar ratio of P:Al is 1.6-3.6:1 as mentioned above, preferably 2-3:1, and has the physicochemical properties such as solid content and viscosity as mentioned above, which can provide the catalytic cracking aid in the catalytic conversion of hydrocarbon oil, match the cracking active component, improve the selectivity of C4 olefins in the product, and obtain a high yield of isobutylene in the liquefied gas product.
[0045] In some embodiments of the present invention, preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of elemental aluminum, aluminum oxide, hydrated aluminum oxide that can be colloided by acid and / or aluminum salts, and can be the above pure substances or a slurry or solution after the pure substances are mixed and slurried with water.
[0046] In the present invention, the elemental aluminum can be selected from at least one of aluminum sheets and aluminum particles; the aluminum oxide can be selected from at least one of γ-alumina, ρ-alumina, χ-alumina, η-alumina, κ-alumina, δ-alumina, and θ-alumina; the acid-colloidable hydrated aluminum oxide can be selected from at least one of gibbsite, diaspore, boehmite, and pseudo-boehmite; the aluminum salt can be selected from at least one of aluminum chloride, aluminum nitrate, and aluminum sulfate.
[0047] Preferably, the aluminum source is pseudo-boehmite.
[0048] In the present invention, the water used as a solvent in the phosphoric acid solution, and the water used as a solvent in the first aluminum source and the second aluminum source, which may be a slurry or a solution, may be acidic water, i.e., decationized water, preferably with a pH value of 3-5, and a sodium oxide content of preferably <5 ppm by mass.
[0049] In some embodiments of the present invention, preferably, the cracking active component is hydrogen type and / or modified Beta zeolite, more preferably modified Beta zeolite, which can be commercially obtained, for example, provided by Qilu Branch of Sinopec Catalyst Co., Ltd. The modified element contained in the modified Beta zeolite is selected from at least one of phosphorus, iron and rare earth elements. The content of the modified element in the modified Beta zeolite is 1-5wt%, preferably 1.1-2wt%. Wherein, the SiO2 / Al2O3 molar ratio of the Beta zeolite is 10-50, preferably 15-30.
[0050] In some embodiments of the present invention, preferably, based on the total dry weight of the catalytic cracking aid, the content of the aluminum phosphate sol is 20-50wt%, preferably 25-45wt%.
[0051] In some embodiments of the present invention, preferably, the clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay, preferably selected from at least one of kaolin, metakaolin and diatomaceous earth.
[0052] The present invention also provides a method for preparing the catalytic cracking aid, comprising: forming a slurry from cracking active components, a binder, clay and water, and obtaining the catalytic cracking aid after drying and roasting.
[0053] In the present invention, the drying temperature is 80-200°C, preferably 80-120°C. The time can be selected according to actual needs, and there is no specific restriction on this. The amount of each component used to form the slurry satisfies the composition of the obtained catalytic cracking aid and meets the composition requirements of the aforementioned catalytic cracking aid, which will not be repeated here. The roasting conditions can refer to the technical conditions in the art, for example, the roasting temperature can be 500-600°C, and the roasting time can be 4-12h.
[0054] The second aspect of the present invention provides a catalytic cracking catalyst, wherein the catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, and the auxiliary agent is the catalytic cracking auxiliary agent provided by the present invention.
[0055] It may also be a catalytic cracking aid prepared by the aforementioned preparation method of the catalytic cracking aid.
[0056] In some embodiments of the present invention, preferably, based on the total weight of the catalytic cracking catalyst, the content of the main catalyst in the catalytic cracking catalyst is 80-95wt%, preferably 85-92wt%; the content of the auxiliary agent is 5-20wt%, preferably 8-15wt%.
[0057] The main catalyst may be a conventional catalytic cracking catalyst in the art, which can be purchased commercially, such as a catalyst with the brand name HBC produced by Sinopec Catalyst Co., Ltd.
[0058] The third aspect of the present invention provides a catalytic cracking aid or a catalytic cracking catalyst provided by the present invention for use in a catalytic reaction of hydrocarbon oil. The hydrocarbon oil can be selected from petroleum and its various fractions, and is particularly suitable for petroleum fractions with a boiling point greater than 330°C, such as one or more of atmospheric residue, vacuum residue, atmospheric wax oil, straight run wax oil, and coking wax oil.
[0059] The fourth aspect of the present invention provides a method for catalytic conversion of hydrocarbon oil, comprising: contacting hydrocarbon oil with the catalytic cracking aid or catalytic cracking catalyst provided by the present invention for reaction. The reaction may be a catalytic cracking reaction, and the reaction conditions may include: a reaction temperature of 350-800°C, preferably 450-650°C; an agent-oil ratio of 2-25, preferably 2-6.
[0060] In the present invention, when the catalytic cracking adjuvant or catalytic cracking catalyst containing the above-mentioned aluminum phosphate sol is used to carry out catalytic cracking reaction, the distribution of products that can be obtained by treating the above-mentioned hydrocarbon oil can increase the propylene yield and the propylene concentration in the catalytic cracking liquefied gas. At the same time, the butene yield, especially the isobutylene yield, can be increased, and the isobutylene concentration in the catalytic cracking liquefied gas can be increased. In particular, when used for catalytic cracking of heavy oil, the product has a higher propylene yield and concentration, and at the same time, the isobutylene yield and concentration are both improved to a certain extent.
[0061] In the present invention, the room temperature is 10-25°C.
[0062] The present invention will be described in detail below by way of examples. The specifications of the raw materials used in the examples are as follows:
[0063] Pseudo-boehmite: Shanxi Jinlu of China Aluminum Corporation, Al2O3 content 66.36wt%;
[0064] Concentrated phosphoric acid: chemically pure, concentration 85wt%, produced by Beijing Chemical Plant;
[0065] Kaolin: solid content 78wt%, produced by Suzhou Kaolin Company;
[0066] Modified Beta zeolite: Na2O is 0.06%, SiO2 / Al2O3 is 21.8, crystallinity is 80%, P content is 2wt%, Sinopec Catalyst Co., Ltd. Qilu Branch;
[0067] Acidic water, decationized water, pH 4.5;
[0068] Industrial catalyst: produced by Sinopec Catalyst Co., Ltd., brand name HBC.
[0069] The components of the catalyst obtained in the examples are determined by calculation based on the feed amounts of the various raw materials.
[0070] Analytical methods:
[0071] (1) The composition of each material was analyzed by XRF fluorescence analysis method (RIPP 117-90 standard method (see "Petrochemical Analysis Method" (RIPP Test Method) edited by Yang Cuiding et al., Science Press, published in 1990)).
[0072] (2) 27 Al-NMR and 31 P-NMR used Varian INOVA II 500MHz superconducting nuclear magnetic resonance spectrometer to test the liquid sample of the prepared aluminum phosphate sol. The experimental conditions were: resonance frequency 130MHz, spectral width 200ppm (mass), sampling times 3000 times, delay time 2s, sampling time 5.6ms, rotation speed 20Hz, and the resonance spectrum was peak-fitted and the peak area was calculated by integration method.
[0073] (3) The size of the colloidal particles was measured using a JEM-2000FX-II transmission electron microscope from Japan Electronics Co., Ltd. The sample was prepared by suspension in distilled water and then quickly fixed by alcohol drying. The accelerating voltage was 120 kV. The average particle size of the colloidal particles was obtained by randomly measuring more than 10 colloidal particle projections in the sample TEM image and taking the average value of the maximum circumscribed circle diameter.
[0074] (4) Viscosity is dynamic viscosity, which was measured using a Thermo Scientific HAAKE VT550 rotational viscometer with a 3# rotor at 20°C and a shear rate of 2900 r / min.
[0075] (5) Stability time: the time during which the prepared aluminum phosphate sol remains in a good sol state at room temperature without stratification.
[0076] In the following examples, the room temperature is 10-25°C.
[0077] Examples 1-5 illustrate the preparation of the aluminum phosphate sol provided by the present invention.
[0078] Example 1
[0079] (1) 53.4 g of phosphoric acid was added to 240 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 27 wt %), and stirred for 10 min. Then 17.8 g of pseudo-boehmite was added, stirred, and the temperature was raised to 55° C. and stirred at 55° C. for 30 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.1, the solid content was 33.6 wt %, and the viscosity was 580 mPa·s);
[0080] (2) 7.6 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 55° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-1.
[0081] Example 2
[0082] (1) 58 g of phosphoric acid was added to 294 g of acidic water and mixed at 20° C. (to obtain a phosphoric acid solution with a concentration of 20 wt %), and stirred for 7 min. Then, 12.9 g of pseudo-boehmite was added, stirred, and the temperature was raised to 75° C. and stirred for 60 min at 75° C. to obtain a first slurry (with a phosphorus-aluminum molar ratio of 6.2, a solid content of 27.4 wt %, and a viscosity of 600 mPa·s);
[0083] (2) 6.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 75° C. for 60 min to obtain an aluminum phosphate sol, which was recorded as PA-2.
[0084] Example 3
[0085] (1) 55.8 g of phosphoric acid was added to 295 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 19 wt %), and stirred for 5 min. Then 17.8 g of pseudo-boehmite was added, stirred, and the temperature was raised to 65° C. and stirred at 65° C. for 45 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.3, the solid content was 27.5 wt %, and the viscosity was 553 mPa·s);
[0086] (2) 4.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 65° C. for 75 min to obtain an aluminum phosphate sol, which was recorded as PA-3.
[0087] Example 4
[0088] (1) 49.7 g of phosphoric acid was added to 241 g of acidic water and mixed at 18° C. (the concentration of the phosphoric acid solution was 21 wt %), and stirred for 5 min. Then, 15.5 g of pseudo-boehmite was added, stirred, and the temperature was raised to 60° C. and stirred at 60° C. for 30 min to obtain a first slurry (the phosphorus-aluminum molar ratio was 4.4, the solid content was 27.7 wt %, and the viscosity was 572 mPa·s);
[0089] (2) 15.5 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 60° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-4.
[0090] Example 5
[0091] (1) 60 g of phosphoric acid was added to 294 g of acidic water and mixed at 20° C. (the concentration of the phosphoric acid solution was 21 wt %), and stirred for 7 min. Then 14.1 g of pseudo-boehmite was added, stirred, and the temperature was raised to 65° C. and stirred at 65° C. for 40 min to obtain a first slurry (with a phosphorus-aluminum molar ratio of 5.8, a solid content of 28.3 wt %, and a viscosity of 650 mPa·s);
[0092] (2) 3 g of pseudo-boehmite was added to the first slurry, and the mixture was stirred at 65° C. for 90 min to obtain an aluminum phosphate sol, which was recorded as PA-5.
[0093] Comparative Example 1
[0094] 21.1 g of pseudo-boehmite (on a dry basis, the same below), 25.8 g of kaolin and 168 g of acidic water were mixed and stirred at 20°C for 30 minutes, 75.6 g of phosphoric acid was added, and then the temperature was raised to 70°C. After the temperature stabilized at 70°C, stirring was continued for 90 minutes to obtain a product recorded as PA-DB-1.
[0095] Comparative Example 2
[0096] 22.3 g of pseudo-boehmite was mixed with 295 g of acidic water at 20°C, stirred and slurried for 30 minutes, 38.6 g of phosphoric acid was poured into the pseudo-boehmite slurry and stirred at 20°C for 30 minutes, and then 20 g of phosphoric acid was added and stirred at 60°C for 90 minutes to obtain a product recorded as PA-DB-2.
[0097] The physicochemical properties of the aluminum phosphate sols obtained in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1, and the TEM image of PA-5 in Example 5 is shown in Figure 1 , PA-1 of Example 1, PA-DB-1 of Comparative Example 1, and PA-DB-2 of Comparative Example 2 31 P-NMR peak fitting diagram is shown in Figure 2 .
[0098] Table 1
[0099]
[0100]
[0101] Note: 1 :Content of aluminum phosphate compound in aluminum phosphate sol
[0102] The phosphate aluminum gel in the present invention 31 P-NMR assignment , where m and n represent the number of Al-OP bonds and POP bonds, respectively. 31 In the P-NMR spectrum, polyhydroxyaluminum phosphate refers to the region with a chemical shift of -8 ppm. and a chemical shift at -13 ppm Monohydroxyaluminum phosphate refers to the chemical shift at -12ppm Hydroxy-free aluminum phosphate refers to the chemical shift at -17ppm The content of each substance is obtained by NUTS peak fitting. The content of polyhydroxy aluminum phosphate refers to and The content of aluminum phosphate compounds (except 0ppm The mass percentage of monohydroxyaluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of hydroxy-free aluminum phosphate is Total aluminum phosphate compounds (except 0ppm The mass percentage of phosphoric acid.
[0103] From Table 1 and Figure 2 It can be seen that compared with the comparative example, the aluminum phosphate sol provided by the present invention and The polyhydroxy aluminum phosphate compound has a high content, the proportion of which is greater than 60wt%, a high hydroxyl content, and good bonding performance. The aluminum phosphate sol provided by the present invention has a long stability time and a high viscosity, and can maintain its good bonding performance for a long time. Moreover, if Figure 1 As shown, the aluminum phosphate sol provided by the present invention has a larger and more uniform particle size, which can reduce the blockage of the molecular sieve pores and acid sites.
[0104] Examples 6-9 illustrate the preparation of the catalytic cracking aid provided by the present invention.
[0105] Example 6
[0106] 50 g of modified Beta zeolite (on a dry basis, the same below) was mixed and slurried in 307 g of water for 20 minutes to obtain a molecular sieve slurry, and then 100 g of kaolin (on a dry basis, the same below) was added and mixed and slurried for 30 minutes. Finally, 50 g of aluminum phosphate sol PA-3 (on a dry basis, the same below) was added and mixed and slurried for 30 minutes to obtain a catalyst slurry.
[0107] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z1. The proportions are shown in Table 2.
[0108] Example 7
[0109] 50 g of modified Beta zeolite was mixed and slurried in 286 g of water for 20 min to prepare a molecular sieve slurry, and then 90 g of kaolin was added and mixed and stirred for 30 min. Finally, 60 g of aluminum phosphate sol PA-3 was added and mixed and stirred for 30 min to prepare a catalyst slurry.
[0110] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z2. The proportions are shown in Table 2.
[0111] Example 8
[0112] 69.8 g of modified Beta zeolite was mixed and slurried in 243.7 g of water for 20 minutes to obtain a molecular sieve slurry, and then 50 g of kaolin was added and mixed and stirred for 30 minutes. Finally, 80 g of aluminum phosphate sol PA-3 was added and mixed and stirred for 30 minutes to obtain a catalyst slurry.
[0113] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z3. The proportions are shown in Table 2.
[0114] Example 9
[0115] 60 g of modified Beta zeolite was mixed in 307 g of water, and then 50 g of kaolin was added and stirred for 30 min. Finally, 90 g of aluminum phosphate sol PA-3 was added and stirred for 30 min to prepare a catalyst slurry.
[0116] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named Z4. The proportions are shown in Table 2.
[0117] Comparative Example 3
[0118] 50 g of modified Beta zeolite (on a dry basis, the same below) was mixed and slurried in 307 g of water for 20 minutes to obtain a molecular sieve slurry, and then 100 g of kaolin (on a dry basis, the same below) was added and mixed and slurried for 30 minutes. Finally, 50 g of aluminum phosphate sol PA-DB-1 (on a dry basis, the same below) was added and mixed and slurried for 30 minutes to obtain a catalyst slurry.
[0119] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named DB1. The proportions are shown in Table 2.
[0120] Comparative Example 4
[0121] 50 g of modified Beta zeolite was mixed and slurried in 307 g of water for 20 min to prepare a molecular sieve slurry, and then 100 g of kaolin was added and mixed and slurried for 30 min. Finally, 50 g of aluminum phosphate sol PA-DB-2 (on a dry basis) was added and mixed and slurried for 30 min to prepare a catalyst slurry.
[0122] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named DB2. The proportions are shown in Table 2.
[0123] Comparative Example 5
[0124] 110 g of modified Beta zeolite (on a dry basis, the same below) was mixed and slurried in 236 g of water for 20 minutes to obtain a molecular sieve slurry. Furthermore, 22 g of pseudo-boehmite (on a dry basis, the same below) and 4.4 g of hydrochloric acid were added and mixed and slurried for 30 minutes. Then, 6 g of kaolin (on a dry basis, the same below) and 8 g of FeCl3 were added and mixed and slurried for 30 minutes. Then, 22 g of aluminum sol (on a dry basis, the same below) was added and mixed and slurried for 30 minutes. 140 g of aluminum phosphate sol PA-3 (on a dry basis, the same below) was added and mixed and slurried for 30 minutes to obtain a catalyst slurry.
[0125] The catalyst slurry was spray dried to prepare a microsphere catalyst, and the microsphere catalyst was calcined at 450°C for 1.5 hours to prepare a catalytic cracking aid containing aluminum phosphate sol, named DB3. The proportions are shown in Table 2.
[0126] Table 2
[0127]
[0128]
[0129] Note: *Modified Beta zeolite, P modified, P content is 2wt%
[0130] Catalyst reaction evaluation method:
[0131] Z1-Z4, DB1-DB3 and industrial catalyst (main catalyst) were mixed in a mass ratio of 1:9 to obtain catalysts C1-C4 and D1-D3. The composition of the industrial catalyst is shown in Table 3.
[0132] Table 3
[0133]
[0134] The composition of the catalytic feedstock oil is shown in Table 4.
[0135] Table 4
[0136]
[0137]
[0138] The catalytic cracking catalysts C1-C4 and D1-D3 prepared above were aged at 800°C and 100% steam for 17 h, respectively, and then filled into a small fixed fluidized bed ACE device (purchased from KTI, USA), with a filling amount of 9 g each. Then, at a reaction temperature of 510°C and a weight hourly space velocity of 12 h -1 The catalyst-oil ratio (weight) was 3, and the catalytic raw oil was injected into the ACE device for catalytic cracking reaction. The reaction results are shown in Table 5.
[0139] The composition of the reaction products is analyzed, including dry gas, liquefied gas, gasoline, diesel, heavy oil and coke, and the catalytic cracking reaction conversion rate of the feedstock oil is calculated according to the following formula:
[0140]
[0141] Liquefied gas contains C4 olefins, which include 1-butene, isobutylene, cis-2-butene and trans-2-butene.
[0142]
[0143]
[0144] Table 5
[0145]
[0146]
[0147] As can be seen from Table 5, the catalytic cracking aid provided by the present invention (such as Examples 7, 8, and 9) contains the provided aluminum phosphate sol. Compared with the comparative examples (Comparative Examples 3, 4, and 5), it is used for the catalytic cracking reaction of heavy oil, and the C4 olefin concentration in the liquefied gas obtained by the catalytic cracking reaction is increased. The catalytic cracking aid has high C4 olefin selectivity and also has a higher isobutylene yield than the comparative example.
[0148] The auxiliary agent provided by the present invention is compared with the auxiliary agent prepared by the aluminum phosphate sol provided by the prior art (Comparative Examples 3 and 4). Under the same formula (other components are the same), the auxiliary agent provided by the present invention (such as Example 6) has a higher C4 olefin yield and selectivity, and has a good economic value. When the aluminum phosphate sol content increases (such as Examples 6, 7, and 8), its C4 olefin yield is improved to a certain extent. And when the molecular sieve content is low (such as Example 9 compared with Example 8), it can also ensure a good C4 olefin yield and selectivity (higher than the comparative example).
[0149] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A catalytic cracking aid, characterized in that: Based on the total dry weight of the catalytic cracking aid, the catalytic cracking aid comprises: 25-35wt% of a cracking active component, 20-55wt% of clay and 20-50wt% of a binder; wherein the binder comprises aluminum phosphate sol; Wherein, the cracking active component is selected from at least one of aluminum phosphate molecular sieve, silicon aluminum phosphate molecular sieve, hydrogen type and / or modified Beta zeolite; the modification is the introduction of at least one of phosphorus, iron and rare earth metal elements into Beta zeolite; The aluminum phosphate sol contains aluminum phosphate compounds containing polyhydroxy aluminum phosphate and monohydroxy aluminum phosphate; based on the total amount of the aluminum phosphate compounds, the content of polyhydroxy aluminum phosphate in the aluminum phosphate compounds is more than 60wt% and the content of monohydroxy aluminum phosphate is less than 20wt%; in the aluminum phosphate sol, based on the total amount of the aluminum phosphate sol, the content of the aluminum phosphate compound is 50-70wt%; in the aluminum phosphate sol, the molar ratio of P:Al is 1.6-3.6:
1.
2. The catalytic cracking aid according to claim 1, wherein Based on the total amount of the aluminum phosphate compound, the content of the polyhydroxy aluminum phosphate in the aluminum phosphate compound is 60-91wt% and the content of the monohydroxy aluminum phosphate is 0.5-20wt%; And / or, in the aluminum phosphate sol, the content of the aluminum phosphate compound is 60-67wt% based on the total amount of the aluminum phosphate sol.
3. The catalytic cracking aid according to claim 2, wherein Based on the total amount of the aluminum phosphate sol, the Al element content is 5-15wt%, and the P element content is 20-30wt%; and / or, in the aluminum phosphate sol, the molar ratio of P:Al is 2-3:1; And / or, the solid content of the aluminum phosphate sol is 20-40wt%; And / or, the viscosity of the aluminum phosphate sol is 1500-7000 mPa·s.
4. The catalytic cracking aid according to claim 3, wherein Based on the total amount of the aluminum phosphate sol, the Al element content is 7-11wt%, and the P element content is 25-27wt%; and / or, the solid content of the aluminum phosphate sol is 21-26wt%; And / or, the viscosity of the aluminum phosphate sol is 2000-4000 mPa·s.
5. The catalytic cracking aid according to any one of claims 1 to 4, wherein: The method for preparing the aluminum phosphate sol comprises: (1) contacting a phosphoric acid solution with a first aluminum source to obtain a first slurry; (2) The first slurry is brought into second contact with a second aluminum source to obtain the aluminum phosphate sol.
6. The catalytic cracking aid according to claim 5, wherein In step (1), the concentration of the phosphoric acid solution is 15-85wt%; And / or, the temperature of the first contact does not exceed 80°C; the time of the first contact is more than 30 minutes; and / or, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus to aluminum molar ratio of the first slurry is 2-10; and / or, the solid content of the first slurry is 25-35wt%; And / or, the viscosity of the first slurry is 500-700 mPa·s.
7. The catalytic cracking aid according to claim 6, wherein In step (1), the concentration of the phosphoric acid solution is 15-30wt%; And / or, the temperature of the first contact is 55-75°C; the time of the first contact is 15-120 minutes; and / or, the phosphoric acid solution and the first aluminum source are added in such an amount that the phosphorus to aluminum molar ratio of the first slurry is 4-7; and / or, the solid content of the first slurry is 27-34wt%; And / or, the viscosity of the first slurry is 550-650 mPa·s.
8. The catalytic cracking aid according to claim 7, wherein In step (1), the first contacting time is 30-60 minutes.
9. The catalytic cracking aid according to claim 5, wherein In step (2), the temperature of the second contact is no more than 80°C; the time of the second contact is more than 30 minutes; and / or, the aluminum introduced by the first aluminum source accounts for 1 / 2-5 / 6 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source; And / or, the first aluminum source and the second aluminum source are each independently selected from at least one of elemental aluminum, aluminum oxide, hydrated aluminum oxide, and aluminum salt.
10. The catalytic cracking aid according to claim 9, wherein In step (2), the temperature of the second contact is 55-75°C; the time of the second contact is 30-120 minutes; And / or, the aluminum introduced by the first aluminum source accounts for 3 / 5-4 / 5 of the total weight of the aluminum introduced by the first aluminum source and the second aluminum source.
11. The catalytic cracking aid according to claim 10, wherein In step (2), the second contact time is 60-90 minutes.
12. The catalytic cracking aid according to any one of claims 1 to 4 and 6 to 11, wherein: The clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.
13. The catalytic cracking aid according to claim 12, wherein: The clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.
14. The catalytic cracking aid according to claim 5, wherein: The clay is selected from at least one of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.
15. The catalytic cracking aid according to claim 14, wherein: The clay is selected from at least one of kaolin, metakaolin and diatomaceous earth.
16. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst comprises: a main catalyst and an auxiliary agent, wherein the auxiliary agent is the catalytic cracking auxiliary agent described in any one of claims 1-15.
17. The catalytic cracking catalyst according to claim 16, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 80-95wt%; and the content of the auxiliary agent is 5-20wt%.
18. The catalytic cracking catalyst according to claim 17, wherein Based on the total weight of the catalytic cracking catalyst, in the catalytic cracking catalyst, the content of the main catalyst is 85-92wt%; and the content of the auxiliary agent is 8-15wt%.
19. Use of the catalytic cracking aid according to any one of claims 1 to 15, or the catalytic cracking catalyst according to any one of claims 16 to 18 in a catalytic reaction of hydrocarbon oil.
20. A method for catalytic conversion of hydrocarbon oil, comprising: The hydrocarbon oil is contacted with the catalytic cracking aid described in any one of claims 1 to 15, or with the catalytic cracking catalyst described in any one of claims 16 to 18 for reaction.
Citation Information
Patent Citations
Phosphorate-containing modified beta-molecular sieve
CN103771437A
Cracking auxiliary agent for increasing low-carbon olefin concentration
CN103785456A
Catalytic cracking additive for increasing concentration of low-carbon olefins and preparation method thereof
CN104998681B
A catalytic cracking aid containing phosphorus-containing and supported metal Beta molecular sieves and its preparation method.
CN107971023B
Process for the preparation of fluid catalytic cracking catalyst additive composition
US6355591B1