A kind of high-aluminum silicate glass and its preparation method and application

By adjusting the component ratio of high-alumina silicate glass and chemical strengthening treatment, the problem of balancing dielectric and mechanical properties in existing technologies has been solved, and protective glass suitable for 5G communication equipment has been prepared.

CN116023024BActive Publication Date: 2024-10-15HEBEI GUANGXING SEMICON TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211648440.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-15
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing high-alumina silicate glass cannot simultaneously meet the requirements of good mechanical properties, low dielectric constant, low dielectric loss, and high matching degree of production process, and therefore cannot meet the high requirements of protective glass for 5G communication equipment.

Method used

By adjusting the component ratios of high aluminosilicate glass, including the molar percentages of SiO2, Al2O3, B2O3, Na2O, Li2O, MgO, CaO, SrO, BaO, ZnO, and P2O5, and controlling the ranges of dielectric factor Y and production factor X, and in conjunction with the use of a clarifying agent, high aluminosilicate glass with low dielectric constant and low dielectric loss is prepared and then subjected to chemical strengthening treatment.

Benefits of technology

The prepared high-alumina silicate glass exhibits excellent mechanical properties after strengthening, effectively reducing 5G high-frequency signal loss. It also has a high degree of compatibility with the production process, making it suitable for protective glass in 5G communication equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004912853530000111
    Figure GDA0004912853530000111
  • Figure GDA0004912853530000112
    Figure GDA0004912853530000112
  • Figure GDA0004912853530000121
    Figure GDA0004912853530000121
Patent Text Reader

Abstract

The present invention provides a high-aluminum silicate glass and a preparation method and application thereof. The high-aluminum silicate glass comprises: 55 mol% to 72 mol% of SiO2, 8 mol% to 25 mol% of Al2O3, 0.1 mol% to 10 mol% of B2O3, 3 mol% to 15 mol% of Na2O, 3 mol% to 15 mol% of Li2O, 0 mol% to 5 mol% of K2O, 0 mol% to 15 mol% of MgO+CaO+SrO+BaO, 0 mol% to 5 mol% of ZnO, and 0.01 mol% to 5 mol% of P2O5; wherein the molar percentage of each component is substituted into a formula to calculate a dielectric factor Y=(SiO2+B2O3) / (Na2O+Li2O+K2O+P2O5)×(MgO+ZnO), and 0.5≤Y≤5.5 is satisfied. The high aluminosilicate glass provided by the present invention has a low dielectric constant and low dielectric loss, can reduce the loss of 5G high-frequency signals, has excellent mechanical properties after strengthening, can provide good protection for 5G communication equipment, and has the advantages of low liquidus temperature and high matching degree with production process. Therefore, the aluminosilicate tempered glass prepared by the present invention can be used as protective glass for various smart mobile devices and other fields requiring excellent mechanical properties of chemically tempered glass materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of glass products, and in particular relates to high-aluminum silicate glass and a preparation method and application thereof. Background Art

[0002] With the rapid development of 5G communication technology, information transmission is moving towards high speed and high frequency. Smartphones, smart wearable devices and tablets are moving towards thinner and more functional while bringing convenience to people's lives. Under this trend, higher requirements are placed on the cover protective glass of smart devices. In the field of display screen protective glass, chemically strengthened high-aluminum silicate electronic glass is usually used. The glass after chemical strengthening has excellent anti-drop and anti-scratch properties; at the same time, the protective glass for high-frequency wireless communication equipment needs to have a lower dielectric constant and dielectric loss to increase signal transmission speed, reduce signal loss, and prevent communication signal distortion. Therefore, high-aluminum silicate glass with low dielectric constant and dielectric loss is the preferred cover protection material in the 5G communication era.

[0003] High aluminosilicate glass usually contains a certain amount of Li2O and Na2O for chemical strengthening, but it will make the glass show a higher dielectric constant and dielectric loss. The commonly used method to reduce the dielectric constant and dielectric loss of glass is to introduce ZrO2 to react with SiO2 to generate low dielectric constant ZrSi x O y However, ZrO2 will make the melting of glass difficult and will aggravate the devitrification trend of glass. In other words, it is difficult for existing cover glass to simultaneously meet the characteristics of good mechanical properties, small dielectric constant, low dielectric loss and high matching degree of production process, and it cannot meet the high requirements for protective glass of 5G communication equipment. Summary of the invention

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a high-aluminum silicate glass. The glass has a low dielectric constant and low dielectric loss, can reduce the loss of 5G high-frequency signals, has excellent mechanical properties after strengthening, can play a good protective role for 5G communication equipment, and has the advantages of low liquidus temperature and high matching degree with the production process. The specific contents are as follows:

[0005] In a first aspect, the present invention provides a high-aluminum silicate glass, wherein the components of the high-aluminum silicate glass include, in terms of molar percentage: 55 mol% to 72 mol% SiO2, 8 mol% to 25 mol% Al2O3, 0.1 mol% to 10 mol% B2O3, 3 mol% to 15 mol% Na2O, 3 mol% to 15 mol% Li2O, 0 mol% to 5 mol% K2O, 0 mol% to 15 mol% MgO+CaO+SrO+BaO, 0 mol% to 5 mol% ZnO, and 0.01 mol% to 5 mol% P2O5;

[0006] Among them, the molar percentage of each component is substituted into the formula to calculate the dielectric factor Y = (SiO2 + B2O3) / (Na2O + Li2O + K2O + P2O5) × (MgO + ZnO), and it satisfies 0.5≤Y≤5.5.

[0007] In some embodiments, the molar percentage of each component is substituted into the formula to calculate the production factor X = (Na2O + Li2O + K2O) × P2O5 / (SiO2 + Al2O3), and 0.1≤X≤0.6 is satisfied.

[0008] In some embodiments, in terms of molar percentage, the molar percentage of each component is substituted into the formula to calculate 1≤(Li2O+Na2O+K2O) / Na2O≤3, 20≤(SiO2+Al2O3) / P2O5≤160.

[0009] In some embodiments, the strengthening parameter Z of the high aluminosilicate glass ranges from 1.5 to 8.2 in mole percentage;

[0010] Z=(Al2O3+B2O3+P2O5) / (RO+ZnO) / Na2O, where RO=

[0011] MgO+CaO+SrO+BaO.

[0012] In some embodiments, the high aluminosilicate glass further contains a clarifier; in terms of mole percentage, the content of the clarifier is no greater than 1 mol %.

[0013] In some embodiments, the fining agent is at least one of a sulfate, a nitrate, a halide, tin oxide, and stannous oxide.

[0014] In some embodiments, the lithium aluminosilicate glass has a dielectric loss of 4.3×10 -3 ~7.2×10 -3 , the dielectric constant is 4.85~6.38.

[0015] In some embodiments, after strengthening, the compressive stress on the glass surface is greater than or equal to 850 MPa, and the Vickers hardness is greater than or equal to 620 kgf / mm 2 For example, the surface compressive stress can be 850MPa, 995MPa, 1022MPa, 1032MPa, 1056MPa, 1078MPa, 1101MPa, and the Vickers hardness can be 620kgf / mm 2 、634kgf / mm 2 、659kgf / mm 2 、668kgf / mm 2 、672kgf / mm 2 .

[0016] In a second aspect, the present invention provides a method for preparing the high alumina silicate glass according to the first aspect, the method comprising:

[0017] According to the formula ratio, the raw materials are fully stirred and mixed to obtain a batch mixture;

[0018] Melting the batch material mixture at high temperature;

[0019] Casting the molten mixture into a mold and annealing it to obtain a glass sheet;

[0020] Mechanically process the glass raw sheet to obtain glass products;

[0021] The glass product is subjected to chemical strengthening treatment.

[0022] In a third aspect, the present invention provides an application of the high-aluminum silicate glass described in the first aspect. Specifically, the application is: applying the high-aluminum silicate glass to cover glass of electronic products.

[0023] The present invention provides a high-aluminum silicate glass and a preparation method and application thereof. The high-aluminum silicate glass comprises: 55 mol% to 72 mol% of SiO2, 8 mol% to 25 mol% of Al2O3, 0.1 mol% to 10 mol% of B2O3, 3 mol% to 15 mol% of Na2O, 3 mol% to 15 mol% of Li2O, 0 mol% to 5 mol% of K2O, 0 mol% to 15 mol% of MgO+CaO+SrO+BaO, 0 mol% to 5 mol% of ZnO, and 0.01 mol% to 5 mol% of P2O5; wherein the molar percentage of each component is substituted into a formula to calculate a dielectric factor Y=(SiO2+B2O3) / (Na2O+Li2O+K2O+P2O5)×(MgO+ZnO), and 0.5≤Y≤5.5 is satisfied. The high aluminosilicate glass provided by the present invention has a low dielectric constant and low dielectric loss, can reduce the loss of 5G high-frequency signals, has excellent mechanical properties after strengthening, can play a good protective role for 5G communication equipment, and has the advantages of low liquidus temperature and high matching degree with the production process. Therefore, the aluminosilicate tempered glass prepared by the present invention can be used as the protective glass of various intelligent mobile devices and other fields of chemically tempered glass materials that require excellent mechanical properties. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. The embodiments of the present invention are described in detail below. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0025] The embodiment of the present invention provides a high-aluminosilicate glass with low dielectric constant and low dielectric loss. The specific contents are as follows:

[0026] In a first aspect, an embodiment of the present invention provides a high-aluminum silicate glass, wherein, in terms of molar percentage, the components of the high-aluminum silicate glass include: 55 mol% to 72 mol% SiO2, 8 mol% to 25 mol% Al2O3, 0.1 mol% to 10 mol% B2O3, 3 mol% to 15 mol% Na2O, 3 mol% to 15 mol% Li2O, 0 mol% to 5 mol% K2O, 0 mol% to 15 mol% MgO+CaO+SrO+BaO, 0 mol% to 5 mol% ZnO, and 0.01 mol% to 5 mol% P2O5;

[0027] Among them, the molar percentage of each component is substituted into the formula to calculate the dielectric factor Y = (SiO2 + B2O3) / (Na2O + Li2O + K2O + P2O5) × (MgO + ZnO), and it satisfies 0.5≤Y≤5.5.

[0028] In this embodiment, the dielectric properties of high aluminosilicate glass are improved by limiting the proportion of each oxide, and the combination of each component enables it to have a low dielectric constant and dielectric loss while having excellent mechanical properties. In specific implementation, the preferred range of the dielectric factor Y is 4.8≥Y≥0.7.

[0029] In this embodiment, SiO2 is a necessary component for forming a network structure. Its addition can improve the heat resistance and chemical durability of the glass, so that the glass can obtain a higher strain point and strength. However, too little SiO2 will deteriorate the main network structure of the glass, increase the dielectric constant of the glass, and deteriorate the mechanical properties and heat resistance of the glass. Too much SiO2 will increase the melting temperature and increase the brittleness, which puts too high requirements on the production process, and is not conducive to chemical strengthening ion exchange, affecting the efficiency of chemical strengthening. Therefore, in order to further improve the comprehensive performance of the prepared glass, preferably, in terms of molar mass percentage, 55mol%≤SiO2≤72mol%. More preferably, in terms of molar mass percentage, 57mol%≤SiO2≤68mol%.

[0030] In this embodiment, Al2O3 acts as a network former, which can promote the integrity of network connection, greatly improve the heat resistance, ion exchange depth, surface compressive stress and mechanical stability of glass, but at the same time, it will make the glass structure tend to be rigid, increase the brittleness of glass, and excessive content will shorten the material properties of glass, making molding difficult, and at the same time, it will cause the glass to be easily devitrified, high-temperature surface tension and high-temperature viscosity are too large, increasing the difficulty of glass production process. The aluminum oxide tetrahedron formed by Al2O3 in glass has a larger volume than the silicon oxide tetrahedron in glass, and the volume of glass expands, thereby reducing the density of glass, providing a strengthening channel for glass in the ion strengthening process, promoting ion strengthening, but will make the dielectric constant of glass larger. When the content is too little, the space of the glass network gap will become smaller, which is not conducive to ion exchange and reduces the efficiency of chemical strengthening. Taking all factors into consideration, based on the molar mass of the composition, the content of Al2O3 is in the range of 8mol% to 25mol% in terms of oxide. Further preferably, in terms of molar mass percentage, 10.5mol%≤Al2O3≤19.5mol%.

[0031] In this embodiment, B2O3, as a glass-forming oxide, can form glass alone. Its addition can enhance the chemical stability and mechanical properties of the glass, reduce the thermal expansion coefficient of the glass, lower the dielectric constant of the glass, and at the same time can accelerate the ion exchange process. B2O3 is also a good flux, which can significantly reduce the glass melting temperature and is also beneficial to the vitrification process. However, when the content of B2O3 is too high, abnormal phenomena will occur, significantly reducing the heat resistance and ion exchange ability of the glass. Considering comprehensively, based on the molar mass of this composition and calculated as oxides, the content of B2O3 is in the range of 0.1 mol% to 10 mol%. Further preferably, in terms of molar mass percentage, 0.5 mol% ≤ B2O3 ≤ 5.7 mol%.

[0032] In this embodiment, P2O5 forms a network by connecting [PO4] tetrahedrons with each other, making the glass network structure loose and the network voids larger, which is beneficial for the mutual diffusion of Na + ions in the glass and K + ions in the molten salt. It plays a promoting role in ion strengthening during the glass strengthening process and is important for obtaining a higher compressive stress layer, but it will increase the dielectric constant of the glass. Therefore, in the preferred case, in terms of molar mass percentage, 0.01 mol% < P2O5 ≤ 5 mol%. Further preferably, in terms of molar mass percentage, 0.15 mol% ≤ P2O5 ≤ 3.2 mol%.

[0033] In this embodiment, Li2O is one of the necessary components of the base glass and belongs to the extra-network component. It can significantly reduce the viscosity of the glass, reduce the melting difficulty of the glass, and at the same time, as the main component of ion exchange, appropriate Li2O can significantly improve the mechanical strength and surface hardness of the glass and increase the ion exchange rate. During the strengthening process, the depth of the compressive stress layer of the glass is increased by ion exchange with Na + in NaNO3 in the molten salt, thereby improving the impact resistance of the glass. Na2O, as an extra-network oxide of the glass, can provide free oxygen to break the silicon-oxygen bond, thereby reducing the viscosity and melting temperature of the glass. Excessive Na2O will reduce the chemical stability and heat resistance of the glass. Na + as a component of ion exchange, exchanges with K +Chemical exchange forms a compressive stress layer on the surface of the glass, increasing the surface compressive stress of the glass. Excessive Na2O is not conducive to the chemical exchange of the glass and affects the strength of the glass after strengthening. K2O has a similar role to Na2O in the glass structure. An appropriate amount of K2O will produce a mixed alkali effect with Na2O, making the glass performance better. Too much K2O will deteriorate the chemical stability of the glass. Therefore, in order to further improve the comprehensive performance of the obtained glass, in terms of molar mass percentage, 3mol%≤Na2O≤15mol%, 3mol%≤Li2O≤15mol%, 0mol%≤K2O≤5mol%. Further preferably, in terms of molar mass percentage, 4mol%≤Na2O≤13.2mol%, 4mol%≤Li2O≤13.2mol%, 0.01mol%≤K2O≤3mol%.

[0034] In this embodiment, MgO and CaO belong to network exo-oxides. MgO has the characteristics of improving the thermal stability of glass and reducing brittleness, which helps to reduce the melting point and high-temperature viscosity of glass. Excessive content will increase the density, increase the incidence of cracks, devitrification, and phase separation, and hinder ion exchange. CaO can relax and break the network structure of glass, and has a melting effect to a certain extent, but too high a content will deteriorate the chemical stability of glass and seriously hinder ion exchange. MgO, CaO, SrO, and BaO are all alkaline earth metal oxides. Their addition can effectively reduce the high-temperature viscosity of glass, thereby improving the solubility and formability of glass, and can increase the strain point of glass. Therefore, in order to further improve the comprehensive performance of the obtained glass, in terms of molar mass percentage, preferably, it contains 0mol% to 15mol% of MgO+CaO+SrO+BaO, and more preferably, 0.01mol%≤MgO+CaO+SrO+BaO≤7.2mol%. More preferably, 0.01 mol % ≤ MgO ≤ 5 mol %, 0 mol % ≤ CaO ≤ 3 mol %, 0 mol % ≤ SrO ≤ 3 mol %, and 0 mol % ≤ BaO ≤ 3 mol %.

[0035] In this embodiment, ZnO has 18 outer electrons. 2+ Ions are more easily polarized, which can reduce the viscosity of glass at high temperatures (such as above 1400°C). When compared with glass without ZnO at the same high temperature, glass containing ZnO has lower viscosity, faster atomic movement, and is less likely to form crystal nuclei, thus reducing the upper limit of the crystallization temperature of the glass. 2+ and Mg 2+The charge number is the same, and the ionic radius is close. When used together, they can produce a similar mixed alkaline earth effect, resulting in the best toughness, chemical resistance and dielectric properties. However, when the ZnO content is too high, the damage and depolymerization effect of ZnO on the glass network structure increases, which is not conducive to reducing the dielectric constant and dielectric loss of the glass. Comprehensively considered, the ZnO content is 0-5mol% in terms of molar mass percentage, and more preferably, in terms of molar mass percentage, 0.01mol%≤ZnO≤3mol%.

[0036] This embodiment uses the coordination between multiple components in a certain ratio, and then the glass product prepared by the process provided by the present invention has a low dielectric constant and low dielectric loss, which can reduce the loss of 5G high-frequency signals. The mechanical properties after strengthening are excellent, which can play a good protective role for 5G communication equipment. At the same time, it has the advantages of low liquidus temperature and high matching degree with the production process. Therefore, the aluminosilicate tempered glass prepared by the present invention can be used as the protective glass of various intelligent mobile devices and other fields of chemically tempered glass materials that require excellent mechanical properties.

[0037] In some embodiments, the molar percentage of each component is substituted into the formula to calculate the production factor X = (Na2O + Li2O + K2O) × P2O5 / (SiO2 + Al2O3), and 0.1≤X≤0.6 is satisfied.

[0038] In specific implementation, the preferred range of the production factor is 0.55≥X≥0.15. In this embodiment, the production factor is set to 0.55≥X≥0.15, so that the final glass has a lower liquidus temperature and devitrification risk, which can highly match the existing production process.

[0039] In some embodiments, the molar percentage of each component is substituted into the formula to calculate 1≤(Li2O+Na2O+K2O) / Na2O≤3 to improve the strengthening performance of the sample; and by making 20≤(SiO2+Al2O3) / P2O5≤160, the difficulty of melting and forming the glass can be reduced.

[0040] In specific implementation, in terms of molar mass percentage, the optimal value range is: 1.3≤(Li2O+Na2O+K2O) / Na2O≤2.8, 30≤(SiO2+Al2O3) / P2O5≤130.

[0041] In some embodiments, the strengthening parameter Z of the high aluminosilicate glass ranges from 1.5 to 8.2 in mole percentage;

[0042] Z=(Al2O3+B2O3+P2O5) / (RO+ZnO) / Na2O, where RO=

[0043] MgO+CaO+SrO+BaO. In this embodiment, the setting of the calculation formula of Z can improve the strengthening performance of the glass product, so that the CS30 and CS50 of the glass product are further improved, thereby achieving better impact resistance.

[0044] In a specific implementation, the preferred range of the strengthening parameter Z of the high aluminosilicate glass is 1.8 to 7.8 in terms of mole percentage.

[0045] In some embodiments, the high aluminosilicate glass further contains a clarifier; in terms of mole percentage, the content of the clarifier is no greater than 1 mol %.

[0046] In some embodiments, the fining agent is at least one of a sulfate, a nitrate, a halide, tin oxide, and stannous oxide.

[0047] In this embodiment, according to different glass preparation processes, the composition may further contain a clarifier for glass melting, and the clarifier is preferably at least one of sulfate, nitrate, halide, tin oxide, and stannous oxide; based on the moles of each component, the content of the clarifier is not more than 1 mol%, preferably 0.05-0.8 mol%. There is no particular limitation on the specific selection of the clarifier, and various selections commonly used in the art may be used, for example, the sulfate may be sodium sulfate, the nitrate may be sodium nitrate and / or potassium nitrate, the chloride may be sodium chloride and / or strontium chloride, and the fluoride may be calcium fluoride.

[0048] In some embodiments, the lithium aluminosilicate glass has a dielectric loss of 4.3×10 -3 ~7.2×10 -3 , the dielectric constant is 4.85~6.38.

[0049] In some embodiments, after strengthening, the compressive stress on the glass surface is greater than or equal to 850 MPa, and the Vickers hardness is greater than or equal to 620 kgf / mm 2 For example, the surface compressive stress can be 850MPa, 995MPa, 1022MPa, 1032MPa, 1056MPa, 1078MPa, 1101MPa, and the Vickers hardness can be 620kgf / mm 2 、634kgf / mm 2 、659kgf / mm 2 、668kgf / mm 2 、672kgf / mm 2 .

[0050] In a second aspect, the present invention provides a method for preparing the high-alumina silicate glass described in the first aspect. The method comprises:

[0051] According to the formula ratio, the raw materials are fully stirred and mixed to obtain a batch mixture;

[0052] Melting the batch material mixture at high temperature;

[0053] Casting the molten mixture into a mold and annealing it to obtain a glass sheet;

[0054] Mechanically process the glass raw sheet to obtain glass products;

[0055] Chemically strengthen glass products.

[0056] In this embodiment, the melting temperature is 1500° C. to 1650° C. and the time is 4 to 8 hours. Those skilled in the art can determine the specific melting temperature and melting time according to actual conditions, which is well known to those skilled in the art and will not be described in detail here.

[0057] In this embodiment, the annealing temperature is 550° C. to 650° C., and the time is 1-3 hours. Those skilled in the art can determine the specific annealing temperature and annealing time according to actual conditions, which is well known to those skilled in the art and will not be described in detail here.

[0058] In this embodiment, there is no particular limitation on the mechanical processing, and various mechanical processing methods commonly used in the art may be used, for example, the product obtained by annealing may be cut, ground, polished, etc.

[0059] In this embodiment, the chemical strengthening treatment includes one chemical strengthening treatment and / or multiple chemical strengthening treatments. Chemical strengthening is achieved by ion exchange on the surface of the glass plate. The chemical strengthening liquid is sodium nitrate, potassium nitrate and / or a mixed molten liquid of the two. The ion exchange temperature is 390°C to 450°C. Those skilled in the art can determine the specific strengthening temperature and molten salt ratio according to actual conditions. This is well known to those skilled in the art and will not be repeated here.

[0060] At room temperature, the dielectric constant at a frequency of 3 GHz is 4.85 to 6.38, and the dielectric loss is 4.3×10 -3 ~7.2×10 -3 After strengthening, the compressive stress on the glass surface is greater than or equal to 850MPa, the compressive stress at a depth of 30μm from the glass surface (CS_30) is greater than or equal to 160MPa, the compressive stress at a depth of 50μm from the glass surface (CS_50) is greater than or equal to 110MPa, the central tensile stress CT is less than or equal to 100MPa, and the four-point bending strength is greater than or equal to 650MPa.

[0061] The high alumina silicate glass provided in the embodiment of the present invention has a dielectric constant of 4.85 to 6.38 and a dielectric loss of 4.3×10 -3 ~7.2×10 -3 Before strengthening, the Young's modulus is greater than or equal to 74Gpa, and the Vickers hardness is greater than or equal to 550kgf / mm 2 After appropriate strengthening treatment, the Vickers hardness is greater than or equal to 620kgf / mm 2 , four-point bending strength exceeds 650MPa, resistance to 180-mesh sandpaper drop height exceeds 160cm, compressive stress (CS_30) at a depth of 30μm from the glass surface is greater than or equal to 160MPa, compressive stress (CS_50) at a depth of 50μm from the glass surface is greater than or equal to 110Mpa, and central tensile stress is less than or equal to 100MPa. The high-alumina silicate glass prepared by the present invention has a low dielectric constant and low dielectric loss, can reduce the loss of 5G high-frequency signals, has excellent mechanical properties after strengthening, can play a good protective role for 5G communication equipment, and has the advantages of low liquidus temperature and high matching degree with the production process.

[0062] In a third aspect, the present invention provides an application of the high-aluminum silicate glass described in the first aspect. Specifically, the application is: applying the high-aluminum silicate glass to cover glass of electronic products.

[0063] The aluminosilicate tempered glass provided by the embodiment of the present invention can be used as the protective glass of various intelligent mobile devices and in other fields where excellent mechanical properties are required for chemically tempered glass materials.

[0064] In order to make those skilled in the art more clearly understand the technical concept of the present invention, the present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. At the same time, in the following embodiments, unless otherwise specified, the materials used can be obtained commercially, and unless otherwise specified, the methods used are conventional methods in the art. The specific contents are as follows:

[0065] In the following examples and comparative examples, the glass density is measured according to ASTM C-693, and the unit is g / cm 3 .

[0066] The thermal expansion coefficient of glass at 50-350°C is measured using a horizontal dilatometer according to ASTM E-228, in units of 10 -7 / ℃.

[0067] The Young's modulus of glass is measured using a material mechanical testing machine according to ASTM C-623, and the unit is GPa.

[0068] According to the test method in ASTM-D150, the glass was sliced, ground and polished, and then its dielectric constant and dielectric loss were tested using a dielectric constant tester.

[0069] According to ASTM E-384, the Vickers hardness of glass is measured using a Vickers hardness tester. The unit is kgf / mm 2 .

[0070] 4PB was measured using a universal testing machine in accordance with ASTM E-1820.

[0071] The glass strain point is measured using an annealing point strain point tester according to ASTM C-336, and the unit is °C.

[0072] The high temperature viscosity-temperature curve of glass was measured using a rotary high temperature viscometer according to ASTM C-965, wherein the molding temperature T4 corresponding to the viscosity of 40000P is in °C.

[0073] The glass liquidus temperature TL is measured in °C using a gradient furnace method according to ASTM C-829.

[0074] The compressive stress on the glass surface was measured using a FSM-6000LE surface stress meter (in MPa).

[0075] The SLP-2000 scattered light stress meter was used to measure the Na+ ion exchange depth (in μm) and central tensile stress (in MPa) of the glass, the compressive stress (in MPa) at a depth of 30 μm from the glass surface, and the compressive stress (in MPa) at a depth of 50 μm from the glass surface.

[0076] Examples 1-36 and Comparative Examples 1-6 were operated according to the following method to prepare the corresponding glass products.

[0077] Weigh each component as shown in Table 1-7, mix well, pour the mixture into a platinum crucible, and then heat it in a 1700℃ resistance furnace for 5 hours, and stir with a platinum rod to expel bubbles. Pour the molten glass into a stainless steel cast iron mold to form a specified block glass product, and then anneal the glass product in an annealing furnace for 2 hours, turn off the power and cool it to 25℃ with the furnace. Cut, grind and polish the glass product, then clean it with deionized water and dry it to obtain a finished glass product with a thickness of 0.7mm. The various properties of each finished glass product were measured separately, and the results are shown in Table 1-7.

[0078] Table 1. Results of testing various properties of the finished glass products obtained in Examples 1-6

[0079]

[0080] Table 2. Results of testing various properties of the finished glass products obtained in Examples 7-12

[0081]

[0082]

[0083] Table 3. Results of testing various properties of the finished glass products obtained in Examples 13-18

[0084]

[0085]

[0086] Table 4. Results of testing various properties of the finished glass products obtained in Examples 19-24

[0087]

[0088]

[0089] Table 5 Results of testing various properties of the finished glass products obtained in Examples 25-30

[0090]

[0091] Table 6 Test results of various properties of the finished glass products obtained in Examples 31-36

[0092]

[0093]

[0094] Table 7. Results of testing various properties of the finished glass products obtained in Comparative Examples 1-6

[0095]

[0096]

[0097] From the performance test results in Tables 1-7 above, it can be seen that the high aluminosilicate glass provided in this embodiment has a dielectric constant of 4.85 to 6.38 at a frequency of 3 GHz at room temperature, and a dielectric loss of 4.3×10 -3 ~7.2×10 -3 Before strengthening, the Young's modulus is greater than or equal to 74Gpa, and the Vickers hardness is greater than or equal to 550kgf / mm 2 After appropriate strengthening treatment, the Vickers hardness is greater than or equal to 620kgf / mm 2, four-point bending strength exceeds 650MPa, resistance to 180-mesh sandpaper drop height exceeds 160cm, compressive stress (CS_30) at a depth of 30μm from the glass surface is greater than or equal to 160MPa, compressive stress (CS_50) at a depth of 50μm from the glass surface is greater than or equal to 110Mpa, and central tensile stress is less than or equal to 100MPa. The high-alumina silicate glass prepared by the present invention has a low dielectric constant and low dielectric loss, can reduce the loss of 5G high-frequency signals, has excellent mechanical properties after strengthening, can play a good protective role for 5G communication equipment, and has the advantages of low liquidus temperature and high matching degree with the production process.

[0098] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.

[0099] The above is a detailed introduction to a high aluminosilicate glass with low dielectric constant and low dielectric loss provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A high alumina silicate glass, characterized in that: In terms of molar percentage, the components of the high alumina silicate glass include: 59.59mol% to 63.58mol% SiO2, 14.21mol% to 17.41mol% Al2O3, 1.65mol% to 3.85mol% B2O3, 6.58mol% to 11.31mol% Na2O, 5.96mol% to 9.25mol% Li2O, 0mol% to 5mol% K2O, 0mol% to 15mol% MgO+CaO+SrO+BaO, 0mol% to 5mol% ZnO, and 0.53mol% to 2.65mol% P2O5; The molar percentage of each component is substituted into the formula to calculate the dielectric factor Y = (SiO2 + B2O3) / (Na2O + Li2O + K2O + P2O5) × (MgO + ZnO), and it satisfies 0.5≤Y≤5.5; In terms of molar percentage, the molar percentage of each component is substituted into the formula to calculate the production factor X = (Na2O + Li2O + K2O) × P2O5 / (SiO2 + Al2O3), and it satisfies 0.1≤X≤0.6; In terms of molar percentage, the molar percentage of each component is substituted into the formula to calculate 1≤(Li2O+Na2O+K2O) / Na2O≤3, 20≤(SiO2+Al2O3) / P2O5≤160; In terms of mole percentage, the strengthening parameter Z of the high aluminosilicate glass ranges from 1.5 to 8.2; Z=(Al2O3+B2O3+P2O5) / (RO+ZnO) / Na2O, where RO= MgO+CaO+SrO+BaO; The dielectric loss of the high aluminosilicate glass at room temperature and a frequency of 3 GHz is 4.3×10 -3 ~7.2×10 -3 , the dielectric constant is 4.85~6.

38.

2. The high alumina silicate glass according to claim 1, characterized in that: The high alumina silicate glass further contains a clarifier; in terms of mole percentage, the content of the clarifier is no more than 1 mol%.

3. The high alumina silicate glass according to claim 2, characterized in that: The clarifier is at least one of sulfate, nitrate, halide, tin oxide and stannous oxide.

4. The high alumina silicate glass according to any one of claims 1 to 3, characterized in that: After strengthening, the compressive stress of the glass surface is greater than or equal to 850MPa, and the Vickers hardness is greater than or equal to 620kgf / mm 2 .

5. A method for preparing high aluminosilicate glass according to any one of claims 1 to 4, characterized in that: include: According to the formula ratio, the raw materials are fully stirred and mixed to obtain a batch mixture; Melting the batch material mixture at high temperature; Casting the molten mixture into a mold and annealing it to obtain a glass original sheet; Mechanically process the glass raw sheet to obtain glass products; The glass product is subjected to chemical strengthening treatment.

6. Use of the high alumina silicate glass according to any one of claims 1 to 4, characterized in that: The high aluminosilicate glass is applied to cover glass of electronic products.